VI.WeldingProceduresandqualifcationsasPerASMESECIXPage1
WELDINGPROCEDURES &QUALIFICATIONS Mostofthepeopleconsidertheweldingqualificationsastotallytheoreticalandhenceitisnotveryuncommontosee
people totally ignoring this aspect in a manufacturing setup. One would often meet several people in the related
industries
unaware
of
difference
between
a
welding
procedure
qualification
and
a
welder
qualification.
This
paper
is
preparedwiththeintentofthrowinglightonaspectsrelatedtotheweldingqualifications.
Whenanitemisdesignedforaparticularapplication,thematerialusedfortheconstructionofsuchanitemisassumed
to have certain properties. Mechanical strength and chemical composition are the two such properties that are
considered very commonly in almost all the engineering designs. Naturally a weldjoint which forms a part of the
componentalso isassumedtohavetheseproperties.Duetotheadvancements intheWeldingTechnologyandNDT
methods ithasbeenpossible toobtain weldjointswhich areasstrongastheparentmaterial.Hence,these days, in
mostcasesweldsareconsideredtohavethestrengthsameasthatofbasematerial.
To check that they have the desired properties, one can carry out any type of tests (either destructive or
nondestructive)fortheparentmetals,inmostofthecases.Butsameisnotthecasewiththeweldmetals.Inmostof
thecases
NDTs
are
the
only
methods
available
for
testing
the
properties.
But
with
NDTs
one
cannot
determine
the
strengthoftheweld.Henceonewouldthinkofmakingasampleoftheweldandtestfortherequiredproperties.This
wouldcallforatesting,foreverynewjobandeverynewjoint.Thisiswheretheconceptofweldingprocedureshelps
onetoreducethenumberoftestsandhencethecost.
WELDINGPROCEDURE: Awelder/weldingengineermustknowseveraldetailsbeforestartingthewelding,suchasbasematerialcomposition,
thickness, process to be used, etc.. These details which a welder/ welding engineer must know before commencing
weldingarecalledWeldingVariables.
Adocument
showing
all
the
applicable
welding
variables
is
called
WPS
(Welding
Procedure
Specification).
ItisnotenoughifonehasonlytheWPS.OnemustensurethattheweldmadeasperWPSmeetsalltherequirements,
whicharenothingbutthepropertiesofthematerialofconstructionassumedbythedesignerwhiledesigningtheitem.
Normally,thepropertiesassumedaremechanicalstrengthandchemicalcomposition.Additionallyitmayalsoinclude
notchtoughness,hardness,corrosionresistanceetc.
Howtoensurethattheweldmadehavetheseproperties?
WeldacouponasperWPSandtest, if itmeetstherequirementsonecanassumethatweldsimilarlymadealsowill
have similar properties. The document in which the actual values of the variables and the results of the test are
recordediscalledaPQR(ProcedureQualificationRecord).Inotherwords,PQRisarecord,whichservesasaprooffor
thesatisfactoryperformanceoftheweldmadeasperthespecificWPSwithinthespecificrangespermitted.
TheaboveprocessoftestingtoensurethepropertiesiscalledProcedureQualificationTest
TheWPS&PQRtogetherconstituteaQualifiedWeldingProcedureorinshortaprocedure.
7/30/2019 09 Welding Procedures and Qualifcations as Per ASME SEC IX
2/7
VI.WeldingProceduresandqualifcationsasPerASMESECIXPage2
Whetheritisrequiredtocarryoutthetestingforeverynewjoint?
No.
Ithas
been
established
that
a
change
in
the
value
of
the
variable
need
not
necessarily
change
the
properties.
Accordinglythevariablesareclassifiedundertwogroups.
Variables,whosechangeresultsinthechangeinthepropertiesarecalledasEssentialVariables. Variables,whosechangedoesnothaveanyeffectontheproperties,arecalledasNonEssentialVariables.
Variables are listed under one more head known as Supplementary Essential Variables. These become essential
variablewhennotchtoughnessisrequiredfortheweldasperapplicablecode.
Nowthatweknow'whataweldingprocedureis',letusunderstandwhatismeantbythequalificationofthewelding
procedure'. One must notice that welding procedure is only a mock up that can represent welding done in a shop
undersimilar
conditions.
But,
in
certain
cases
where
lesser
factor
of
safety
is
considered
this
may
not
be
sufficient.
Hence, most of the codes call for a production weld coupons as an additional measure. One must note that these
productioncouponsthemselvesalsoactasqualificationtestsfortheweldingprocedures.
WELDERQUALIFICATION: Welderqualificationisthesecondtypeofqualificationrequired.
Itisverymuchsimilartoadrivinglicenseissuedtothedrivers. Thisauthenticatesapersontoperformwelding.Justas
a person capable of manipulating a steering wheel, brakes, clutch etc., can act as a driver, a person capable of
depositingsoundweldmetalcanbecomeawelder. Whatisrequiredforawelderisskilltodepositsoundweldmetal
byproperly
interpreting
the
welding
procedure.
A
document
similar
to
driving
license
authorizing
the
driver
to
drive
is
theWPQ(WelderPerformanceQualificationrecord)forthewelder.Theprocessoftestingthecapabilityofthewelderisknownas"WelderPerformanceQualificationtest".Onemustnoticethatmostofthecodesallowwelderqualificationonthejobsignifyingthefactthatwhatisimportant
isthesoundnessoffinalweld.Hence,onemustviewWelderQualificationmoreasatooltogetarepairfreejointin
thefirstinstance.
INTRODUCTIONTO
SEC
IX
OF
ASME
Throughoutthispaperareference ismadetoASMEboilerandpressurevesselcodeforthesakeofconvenience.But
thediscussionsarenormallyvalidforanycodes.
SECIXofASMEcoversvariousaspectsrelatingtotheweldingqualifications.Thefollowingpointsmustclarifysomeofthedoubts/confusionscommonlyseeninthebeginners.
7/30/2019 09 Welding Procedures and Qualifcations as Per ASME SEC IX
3/7
VI.WeldingProceduresandqualifcationsasPerASMESECIXPage3
1. Thissectionmustbereferredonlywhenthedesigncode(suchasSECVIIIdiv.1),crossreferstothissection2. Thissectiondoesnotguideintheselectionofelectrode3. Thissectiondoesnotguideinthedesignofjoints4. Thissectiondoesnotspecifythetypeandextentofradiography/NDTtobeused5. Thissectiondoesnotspecifytheacceptancecriteria(i.e.typesandextentofdiscontinuitiesacceptable).6.
This
section
does
not
specify
Energy
value
for
impact
testing
For points specified in 3, 4, 5 and 6 one must refer the Design code. Knowledge of how the contents (and their
organization)ofSECIXshouldgreatlyhelpthereaderstosolvethecommonlyseenstartingtrouble.
Thissectionhastwoparts,weldingandbrazing.Under Welding,thereare4chapters(Article ItoIV), inadditionto
initialintroduction.
ArticleI:General.Mainlycovers
Positionsofwelding Examinations(VariousTypesofTests,TestingProcedures,SpecimenDetails,AcceptanceCriteria)etc.
ArticleII WeldingProcedureQualifications WPS,PQR Theircontents,Format Listofvariables Qualifiedranges Typeandnumberofexaminationsrequired
ArticleIII WeldingPerformanceQualifications WPQ ListofVariables Qualifiedranges Typeandnumberofexaminationsrequired
ArticleIV CompiledweldingdatameantforusingwitharticlesI,II,III
Hence,forexample,onewhowantstoqualifyaweldercandirectlyreferarticleIII.
FollowingTipsmusthelpreaderwhenreadingtheweldingdata:
NeverreadtheweldingdatagiveninarticleIVunlesscalledupontodosobyarticlesI,IIorIII Normally adding "a new qualification shall be done when " before reading data against essential variable
givenin
the
tables
of
Article
II
and
III(such
as
QW
253/6),
makes
the
reading
easy
Normallyadding"anewqualification isnotrequiredwhen"beforereadingthedataagainstnonessentialvariablegiveninthetablesofarticleII(suchasQW253/6),makesthereadingeasy
7/30/2019 09 Welding Procedures and Qualifcations as Per ASME SEC IX
4/7
VI.WeldingProceduresandqualifcationsasPerASMESECIXPage4
ThicknessofthetestcouponThicknessselectionistheimportantandmostlyconfusedparameter
WeldingprocedureFollowing
parameters
shall
be
considered
in
the
selection
of
thickness
Testcouponthickness governstherange Impactrequirement governsthelowerlimit Normalizingrequirement governstheupperlimit
AppendixIdescribesthicknessselectioninmoredetail.
WeldersQualificationOnemustpreferablyqualifyawelderwithacouponof20mmthicknessormorewhichwillqualifyhimtowelddeposit
ofanythickness.
GroupingofmaterialsBase materials and electrodes / filler materials are grouped variously due to their similarity of
composition, mfg., Practice etc., to reduce the number of qualification tests to be carried out.
Belowwewilldiscussfewofthem.
BasemetalsPnumber
This is the grouping of BaseMaterials based on their chemical composition, weldability mechanicalproperties etc. P
standsfor
Parent
metal.
Table
QW422
lists
the
P
numbers
of
various
materials.
QW422
and
QW424
describe
the
rules
for usingthe P numbers ofqualifications.With thehelpof Pnumbersthenumberof qualificationtestsrequiredare
greatlyreduced.Forexampleallplaincarbonsteels(SA105,SA106,SA515,SA516etc.)areassignedaPnumberof1.
GnumberThisisasubgroupingofferrousBaseMaterialshavingspecifiedimpacttestrequirements,withinaPnumber.Gstands
for Group. Table QW422 lists the G numbers of various materials. This willbe an additionalrestriction on P number
whenimpacttestingisrequiredforthebase/weldmetalinthejobspecification.
AsimpleexampleofusageofPnumberandgroupnumberisasfollows
A
procedure
qualified
using
a
plates
confirming
to
SA516
Gr.60
can
be
used
to
weld
ajoint
between
the
pipes
confirmingtoSA106Gr.Bassumingthatallotherparametersremainunaffected.
In the WPS it is enough if only P number and group number are specified. When they are not known, material
specificationshallbewritten(ex..ifbasematerialIS2062).Whenspecificationalsoisnotknown,chemicalcomposition
shallbewritten.Thelatteroptionsactuallyreducetherangequalified
7/30/2019 09 Welding Procedures and Qualifcations as Per ASME SEC IX
5/7
VI.WeldingProceduresandqualifcationsasPerASMESECIXPage5
FillermaterialsFnumberThis
is
the
grouping
of
electrodes
and
filler
materials
based
on
their
usability
characteristics
mainly
governed
by
flux
or
shielding medium used (which also govern their electrical characteristics). F stands for F Filter metal. These aredescribedinQW430
AnumberThis is the grouping of electrodes and filler materials based on the weld metal chemical composition. 'A' stands for
weldmetalAnalysis.ThesearedescribedinQW440
SomefactsrelatingtoWPS,PQR,WPQ Adoublewelded(weldedfromboththesides)jointisconsideredasajointwithbacking.Weldmetalbecomes
theBackingmaterial.
Size of base metal, normally designated as T and size of weld deposit normally designated as t must beconsideredseparately.
WPS/PQR A procedure qualified using plates can be used for welding the pipes, provided the P number G number
criteriaismet.
Aprocedurequalifiedinanyonepositioncanbeusedtoweldinanyotherpositionprovidedjobspecificationsdo
not
specify
impact
test.
Aprocedurequalifiedusinggroveweldscanbeusedforfilletweldsofanysize. Onemustalwayscarryout impacttestingatthe lowestpossibletemperature, intheprocedurequalification
test.Thiscanbeusedforthejobshavingimpactrequirementornot
Technically,aprocedurequalificationtest,whichhasfailedtomeettherequiredtensilestrengthcanbeusedforjobswithmaterialsoflowerstrength.Forexample,ifthetensiletestresultsshowedavalueof65ksiwhen
testedwithacouponmaterialofSA516Gr.70,E7018electrode,onnormalizingcanbeusedforweldsmade
onequipmentofSA516Gr.60,provided,allotherparametersremainsame
A test coupon of thickness 40mm used for procedure qualification test covers largest range from 5 mm to200mm(withoutheattreatmentorimpactrequirements).
TheformatrecommendedbySECIX,commonlyusedforWPS/PQR,iscommonforprocessesSMAW,GTAW,SAW
and
GMAW.
Hence,
one
must
be
careful
when
using
them,
since,
some
of
the
points
are
not
applicable
forsomeprocesses.
WPQ Normallyaweldercanbequalifiedusingonlyaradiographictest. Achangeoffillermetal(Fnumber)needsarequalificationofwelder
7/30/2019 09 Welding Procedures and Qualifcations as Per ASME SEC IX
6/7
VI.WeldingProceduresandqualifcationsasPerASMESECIXPage6
Presence or absence of impact test or normalizing does not affect the welder's skill and hence thequalification.
A small diameter pipe requires more skill for welding. Hence, a welder qualified on lower diameters canalwaysweldhigherdiameters(plateisapipewithinfinitediameter).
7/30/2019 09 Welding Procedures and Qualifcations as Per ASME SEC IX
7/7
VI.WeldingProceduresandqualifcationsasPerASMESECIXPage7
AppendixIDeterminationoftestcouponthicknessforweldingprocedurequalification
IdeallyonemuststartwithtablessuchasQW253/256,proceedtoweldingdatasuchasQW403.8(asspecifiedinthe
tables)andthenproceedtoQW451(asspecified inthedata) andselectthethickness insuchawayastocoverthe
largestrange.
Letustakeanexampletoillustratetheabovepoint.Forthejointconfigurationshownontheright,variousstepstobe
followedtoarriveattheoptimumthicknessareasfollows.
Step1: Startwiththicknesssameasthejob.But,codedoesnotpermitdissimilarthicknessforthetestcouponStep2: Choose16mm(arbitrary),Thiswillqualifyusfor,Reference Thickness
Tofbasemetal tofweldmetal,max
From To GTAW SMAW
AsperQW450(BasedonThicknessofthecoupon) 5 32 16 16
AsperQW407.4(duetonormalizing) 18 8.8 8.8
AsperQW403.6(duetoimpacttestrequirement) 16
Result 16 18 8.8 8.8
Step3: Choose32mm(arbitrary).ThiswillqualifyusforReference Thickness
Tofbasemetal tofweldmetal,max
From To GTAW SMAW
AsperQW450(BasedonThicknessofthecoupon) 5 64 64 64
AsperQW407.4(duetonormalizing) 35 35 35
AsperQW403.6(duetoimpacttestrequirement) 16
Result 16 35 35 35
Onemustnotethatthestep3givesusthelargestrange.Onemay,however,chooseanythicknesshigherthan32mm,
but this would not yield any additional benefit due to the presence of normalizing in thejob requirement in this
example.AdditionallyQW407.2indirectlyrestrainsusfromchoosingathicknessvaryingtoomuchfromthatofjob.
Whathappens
when
a
production
weld
has
two
dissimilar
metal
thicknesses?
This
shall
be
arrived
at
in
two
steps
1. ThicknessofthethinnermembershallbeaspermittedbyQW4512. Thicknessofthethickermembershallbe
i. Unlimitedforspecifiedmaterialprovideda) MaterialsareofsamePnumber.b) qualificationismadeon>
ii. limitedwithintherangeofqw451***********
Process(assumption) 2layers(root
andhotpass)ofGTAWandrestby
SMAW(fillupandfinal).
Heattreatment Normalizing
Min.designtemperature. 48C
16 32SS CS
Recommended