Chapter 8 §8.3 Waterproof Sheet Introduction Introduction Polymer Modified Polymer Modified Asphalt Sheet Material Asphalt Sheet Material Polymer Water Proof Polymer Water Proof Sheet Sheet

Chapter 8 §8.3 Waterproof Sheet Introduction Polymer Modified Asphalt Sheet Material Polymer Water Proof Sheet

Embed Size (px)

Citation preview

Page 1: Chapter 8 §8.3 Waterproof Sheet Introduction Polymer Modified Asphalt Sheet Material Polymer Water Proof Sheet

Chapter 8 §8.3 Waterproof Sheet

IntroductionIntroductionPolymer Modified Asphalt Sheet Polymer Modified Asphalt Sheet

MaterialMaterialPolymer Water Proof SheetPolymer Water Proof Sheet

Page 2: Chapter 8 §8.3 Waterproof Sheet Introduction Polymer Modified Asphalt Sheet Material Polymer Water Proof Sheet

SBS Modified Asphalt Sheet Material—Elastomer Asphalt Sheet Material

APP Modified Asphalt Sheet Material—Plastomer Asphalt Sheet Material

Polymer Modified Asphalt Sheet Material

Page 3: Chapter 8 §8.3 Waterproof Sheet Introduction Polymer Modified Asphalt Sheet Material Polymer Water Proof Sheet

SBS modified asphalt waterproof sheet is a kind of waterproof sheet material formed by dipping support with SBS modified asphalt. It is sprayed plastic asphalt on both sides, with sewing fine sand, mineral particles or covering polyethylene film on the upper side and at the bottom.

It belongs to elastomer sheet (thermoplastic plastomer).

Both fiberglass and polyester texture can be used as the support.

Definition

SBS Modified Asphalt Waterproof sheet

Page 4: Chapter 8 §8.3 Waterproof Sheet Introduction Polymer Modified Asphalt Sheet Material Polymer Water Proof Sheet

Fig.8.3.3 SBS Modified Asphalt Waterproof Sheet

SBS Modified Asphalt Waterproof sheet

Page 5: Chapter 8 §8.3 Waterproof Sheet Introduction Polymer Modified Asphalt Sheet Material Polymer Water Proof Sheet

Tab, Grade and PropertyTab, Grade and PropertyAccording to JC/T560-2001,the

number of sheet is based on the weight of 10 ㎡ sheet.

The sheet of fiberglass support can be divided into three grades:20,35 and 45.

The sheet of polyester felt support can be divided into four grades:25, 35, 45 and 55.

Page 6: Chapter 8 §8.3 Waterproof Sheet Introduction Polymer Modified Asphalt Sheet Material Polymer Water Proof Sheet

The sheet can be divided into three grades by its physical properties.

the qualified rate the first rate the top rate

The grade and physical properties of the second kind of support conform with the stipulation of table 8.3.1 and table 8.3.2.

The test instruments are shown in Fig.8.3.5

Tab, Grade and PropertyTab, Grade and Property

Page 7: Chapter 8 §8.3 Waterproof Sheet Introduction Polymer Modified Asphalt Sheet Material Polymer Water Proof Sheet

serial numbe

r

tab 25 35 45

grade

name of tab

the top rate

the first rate

the qualif-ie

d

the top rate

the first rate

the quali-f

ied

the top rate

the first rate

the quali-fie

d

1content of soluble matter at

least1300 2100 2900

2Imper-meabili

ty

pressure ≥0.15 ≥0.20 ≥0.20

continuous time ≥30

3 heat resistance ability100 90 100 90 100 90

heated for 2h, the coating should not be mobile

4tension at least

longitudinal section

400 350 300 400 350 300 400 350 300

cross section 300 250 200 300 250 200 300 250 200

5 elasticity

-25 -20 -15 -25 -20 -15 -25 -20 -15

R=15mm,3S, 180°, without cracks R=25mm3S, 180°, without cracks

Tab.8.3.1 Technical property of fiberglass support plastomer

asphalt waterproof sheet

Page 8: Chapter 8 §8.3 Waterproof Sheet Introduction Polymer Modified Asphalt Sheet Material Polymer Water Proof Sheet

tab 25 35 45 55

grade

tab

the top rate

the first rate

the quali-fie

d

the top rate

the first rate

the quali-f

ied

the top rate

the first rate

the quali-f

ied

the top rate

the first rate

the quali-fie

d

content of soluble matter at least

1300 2100 2900 3700

Imperme-ability

pressre ≥0.30

continu-ous ti

me≥30 ( min )

heat resistance ability

100 90 100 90 100 90 100 90

heated for 2h, the coating should not be mobile

tension at least 800 600 400 800 600 400 800 600 400 800 600 400

elongation of facture

40 30 20 40 30 20 40 30 20 40 30 20

elasticity-25 -20 -15 -25 -20 -15 -25 -20 -15 -25 -20 -15

R=15 ㎜ ,3S, 180°, without cracks R=25 ㎜ ,3S, 180°, without cracks

Tab.8.3.2 Technical property of polyester felt support elastomer asphalt waterproof sheet material

Page 9: Chapter 8 §8.3 Waterproof Sheet Introduction Polymer Modified Asphalt Sheet Material Polymer Water Proof Sheet

Fig.8.3.4 Test instruments Fig.8.3.4 Test instruments

Tension instrumentTension instrument

Tension specimenTension specimen

Instrument for Instrument for impermeabilityimpermeability

Page 10: Chapter 8 §8.3 Waterproof Sheet Introduction Polymer Modified Asphalt Sheet Material Polymer Water Proof Sheet

It is widely used in all kinds of waterproof It is widely used in all kinds of waterproof and damp proofing projects, especially in coland damp proofing projects, especially in cold areas and frequently distorted buildings. d areas and frequently distorted buildings.

Tab 35 and its belowings can be used in mTab 35 and its belowings can be used in multi-layer water proofing.ulti-layer water proofing.

Tabs above tab 35 can be used in unique-lTabs above tab 35 can be used in unique-layer water proofing and multi-layer water prayer water proofing and multi-layer water proofing as well as in heat construction.oofing as well as in heat construction.

SBS Modified Asphalt Waterproof sheet

ApplicationApplication

Page 11: Chapter 8 §8.3 Waterproof Sheet Introduction Polymer Modified Asphalt Sheet Material Polymer Water Proof Sheet

APP modified asphalt waterproof sheet is one kind APP modified asphalt waterproof sheet is one kind of plasticity asphalt waterproof sheet, formed by dippiof plasticity asphalt waterproof sheet, formed by dipping support with asphalt or thermal elastic (atactic polng support with asphalt or thermal elastic (atactic polypropylene) modified asphalt (elasticity asphalt in shoypropylene) modified asphalt (elasticity asphalt in short). rt). Spraying plastic asphalt on both sides , sewing fine Spraying plastic asphalt on both sides , sewing fine sand, mineral particles or covering polyethylene film osand, mineral particles or covering polyethylene film on the upper side .n the upper side .Sewing fine sand or covering polyethylene film at thSewing fine sand or covering polyethylene film at the bottom. e bottom.

APP Modified asphalt Waterproof Sheet

DefinitionDefinition

Page 12: Chapter 8 §8.3 Waterproof Sheet Introduction Polymer Modified Asphalt Sheet Material Polymer Water Proof Sheet

APP Modified asphalt Waterproof Sheet

Fig8.3.5 APP Modified Asphalt Waterproof Sheet

Page 13: Chapter 8 §8.3 Waterproof Sheet Introduction Polymer Modified Asphalt Sheet Material Polymer Water Proof Sheet

Tab, Grade and Property

According to JC/T559-2001,the number of sheet is based on the weight of 10 ㎡ sheet.

The sheet of fiberglass support can be divided into three grades: 20,35 and 45.

The sheet of polyester felt support can be divided into four grades:25,35,45 and 55.

Page 14: Chapter 8 §8.3 Waterproof Sheet Introduction Polymer Modified Asphalt Sheet Material Polymer Water Proof Sheet

The sheet can be divided into three grades by its physical propertiesthe qualified ratethe first ratethe top rate

The grade and physical properties of the second kind of support conform with the stipulation of the following form.

Tab, Grade and Property

Page 15: Chapter 8 §8.3 Waterproof Sheet Introduction Polymer Modified Asphalt Sheet Material Polymer Water Proof Sheet

tab 25 35 45

grade

name of tab

the top rate

the first rate

the qualified

the top rate

the first rate

the qualified

the top rate

the first rate

the quali

-fied

content of soluble matter at least

1300 2100 2900

imp-ermeability

pressure ≥0.15 ≥0.20 ≥0.20

continuous time

≥30 ( min )

heat resistance ability

130 120 110 130 120 110 130 120 110

heated for 2h, the coating should not be mobile

tension at least 400 350 300 400 350 300 400 350 300

elongation of facture 300 250 200 300 250 200 300 250 200

elasticity

-15 -10 -5 -15 -10 -5 -15 -10 -5

R=15mm3S, 180°, without cracksR=25mm,3S, 180°,

without cracks

Tab.8.3.3 Technical property of fiberglass support plastomer

asphalt waterproof sheet material

Page 16: Chapter 8 §8.3 Waterproof Sheet Introduction Polymer Modified Asphalt Sheet Material Polymer Water Proof Sheet

tab 35 45 55

grade

name of tab

the top rate

the first rate

the qualif

ied

the top rate

the first rate

the qualif

ied

the top rate

the first rate

the qualif

ied

content of soluble

matter at least

2100 2900 3700

impermeability

pressure

≥0.30

continuous time

≥30 ( min )

heat resistance

ability

130 120 110 130 120 110 130 120 110

滑动 heated for 2h, the coating should not be mobile

tension at least

800 600 400 800 600 400 800 600 400

elongation of facture

40 30 20 40 30 20 40 30 20

elasticity

-15 -10 -5 -15 -10 -5 -15 -10 -5

R=15 ㎜ ,3S, 180°, without cracks

R=25 ㎜ ,3S, 180°, without cracks

Tab.8.3.4 Technical property of polyester felt plastomer asphalt waterproof sheet material

Page 17: Chapter 8 §8.3 Waterproof Sheet Introduction Polymer Modified Asphalt Sheet Material Polymer Water Proof Sheet

Application

It is widely used on all kinds of water proofing and damp proofing projects, especially in areas at high temperature or in strong solar radiation.

Tab 35 and its belowings can be used in multi-layer water proofing

Tabs above tab 35 can be used in unique-layer water proofing and multi-layer water proofing as well as in heat construction

Besides the two kinds of materials, polymer modified asphalt waterproof sheet material also contains other kinds of polymer and supports with different properties and ranges in water proofing.

APP modified asphalt waterproof sheet

Page 18: Chapter 8 §8.3 Waterproof Sheet Introduction Polymer Modified Asphalt Sheet Material Polymer Water Proof Sheet

Property

Heat resistance

Flexibility

Water impermeability

APP modified asphalt waterproof sheet material

Physical PropertiesPhysical Properties