16
ACC Concrete FOAMED CONCRETE SURAJ GOYAL DET 2013 NOV. GREATER NOIDA DELHI

Presentation Of Foamcrete

Embed Size (px)

Citation preview

Page 1: Presentation Of Foamcrete

ACC Concrete

FOAMED CONCRETE

SURAJ GOYAL

DET 2013 NOV.

GREATER NOIDA

DELHI

Page 2: Presentation Of Foamcrete

ACC Concrete

INTRODUCTION

Foam Concrete is also Known as " Cellular light weight

concrete", "CLC", "Foamed cement", "Light Weight

Concrete" across the world with its greater advantages

from 5 years.

The synonyms are:

o Aerated concrete

o Lightweight concrete

o Porous concrete

Page 3: Presentation Of Foamcrete

ACC Concrete

DENSITY 300-500 KG/M3 MADE WITH

CEMENT & FOAM ONLY

Foam concrete with this densities is used in roof

and floor as insulation against heat and sound

and is applied on rigid floors (i.e. in itself it is not a

structural material). It is used interspace filling

between brickwork leaves in underground walls,

insulation in hollow blocks and any other filling

situation where high insulating properties are

required.

Page 4: Presentation Of Foamcrete

ACC Concrete

DENSITY 600-900 KG/M3 MADE WITH

SAND, CEMENT & FOAM

Used for the manufacture of precast blocks and

panels for curtain and partition walls, slabs for

false ceilings, thermal insulation and

soundproofing screeds in multi-level residential

and commercial buildings. Foam concrete of this

density range is also ideal for bulk fill application.

Page 5: Presentation Of Foamcrete

ACC Concrete

TRIALS CONDUCTED IN LAB

2-Jun-14

Foamcrete- Trial With Rohini Foam (1:30) 0.02

Material Qty Specific Gravity Volume Moisture Absorption SSD Batch Qty

OPC 250 3.15 79.37 250.00 5.00

Fly Ash 400 2.20 181.82 400.00 8.00

Water 170 1.00 170.00 170.00 3.40

Foam 65.44 65.44 0 0 0.00 1.31

496.62

W/C 0.26 17.71

DENSITY OF FOAM CRETE=867.66 KG/M3

WATER ADD=750 GM

Page 6: Presentation Of Foamcrete

ACC Concrete

TRIALS CONDUCTED IN LAB

4-JUN 2014

Foamcrete- Trial With Rohini Foam (1.5:25)

0.02

Material Qty Specific Gravity Volume Moisture Absorption SSD Batch Qty

OPC 250 3.15 79.37 250.00 5.00

Fly Ash 400 2.20 181.82 400.00 8.00

Water 220 1.00 220.00 220.00 4.40

Foam 46.66 46.66 0 0 0.00 0.93

527.84

W/C 0.34 18.33

DENSITY OF FOAM CRETE=1134 KG/M3

Page 7: Presentation Of Foamcrete

ACC Concrete

TRIALS CONDUCTED IN LAB

10-Jun-14

Foamcrete- Trial With Cemairin (1:30)

0.02

Material Qty Specific Gravity Volume Moisture Absorption SSD Batch Qty

OPC 250 3.15 79.37 250.00 5.00

Fly Ash 400 2.20 181.82 400.00 8.00

Water 220 1.00 220.00 220.00 4.40

Foam 39.22 39.22 0 0 0.00 0.78

520.40

W/C 0.34 18.18

DENSITY OF FOAM CRETE=845 KG/M3

Page 8: Presentation Of Foamcrete

ACC Concrete

TRIALS CONDUCTED IN LAB

14-Jun-14

Foamcrete- Trial With Cemairin (1:30)

0.02

Material Qty Specific Gravity Volume Moisture Absorption SSD Batch Qty

OPC 250 3.15 79.37 250.00 5.00

Fly Ash 400 2.20 181.82 400.00 8.00

Water 220 1.00 220.00 220.00 4.40

Foam 44.78 44.78 0 0 0.00 0.90

525.96

W/C 0.34 18.30

DENSITY OF FOAM CRETE=870 KG/M3

Page 9: Presentation Of Foamcrete

ACC Concrete

Page 10: Presentation Of Foamcrete

ACC Concrete

Page 11: Presentation Of Foamcrete

ACC Concrete

SITE VISIT

Page 12: Presentation Of Foamcrete

ACC Concrete

Page 13: Presentation Of Foamcrete

ACC Concrete

MIXER AT SITE

Page 14: Presentation Of Foamcrete

ACC Concrete

FOAMCRETE AT SITE

Page 15: Presentation Of Foamcrete

ACC Concrete

ADVANTAGES OF FOAMCRETE

Foam gross density adjustable.

Low cost.

High yield mortar / concrete

Non-toxic

Reduces the dead load of the structure.

Fire resistant.

Wall insulation in multi-storey buildings.

Page 16: Presentation Of Foamcrete

ACC Concrete

THANK YOU