8/13/2019 Welding Procedure for pipes
http://slidepdf.com/reader/full/welding-procedure-for-pipes 1/5
WELDING PROCEDURE SPECIFICATION
NO. 1/8-32-1
FOR
GAS TUNGSTEN ARC WELDING (GTAW)
AND
SHIELDED METAL ARC WELDING (SMAW)
OF
CARBON STEEL PIPE WITH STAINLESS STEEL CLADDING
USING ER317L and E317L-15 or -16 FILLER METALS
THIS DOCUMENT IS THE PROPERTY OF
_______________________________
(Company)
Jointly Developed With The NATIONAL CERTIFIED PIPE WELDING BUREAU
1385 Piccard Drive
Rockville, MD 20850
8/13/2019 Welding Procedure for pipes
http://slidepdf.com/reader/full/welding-procedure-for-pipes 2/5
This Welding Procedure Specification (WPS) and supporting Procedure Qualification record(s)
(PQR) are the property of the National Certified Pipe Welding Bureau. They are issued for
adoption by members only and are to be returned to the Bureau upon termination of
membership
ANSI American National Standards Institute
ASME American Society of Mechanical Engineers
AWS American Welding Society, Inc.
REPRODUCTION AND USE OF THIS WPS AND SUPPORTING PQR(S) BY OTHER THAN
MEMBERS OF THE BUREAU IS UNAUTHORIZED
© 2005-Copyrighted in the United States and Canada by the National Certified Pipe Welding Bureau
Jointly Developed with the
National Certified Pipe Welding Bureau
1385 Piccard Drive
Rockville, MD 20850-4340
8/13/2019 Welding Procedure for pipes
http://slidepdf.com/reader/full/welding-procedure-for-pipes 3/5
Base Metals (QW-403)
P/S Number 1 clad with 8 Group No.1 and 2
to P/S Number 1 clad with 8 Group No.1 and 2
(written for P-1 pipe lined with P-8 clad)
Base Metal Thickness Range
Groove Welds: 3/16 to 1.1 in*.
Fillet welds: Not permitted
Minimum Outside Diameter
Groove Welds: All GTAW, 1” SMAW
Fillet Welds: Not permitted
*includes cladding thickness of 10% up to 0.10”
Filler Metals and Electrodes (QW-404) Root and Fill Fill
Specification Number: SFA 5.9* SFA5.5
AWS Classification: ER317L E317L-15 or
F-number: 6 5
A-Number: N/A N/A
Maximum Weld Metal Thickness:
Grooves: 0.40” 0.70”
Fillets: None None
Maximum Bead thickness: 1/8” 1/8”
Supplemental Filler Metal: N/A N/A
Consumable Insert: Optional* N/APulsed Power Supply: Optional Not permitte
Penetration-enhancing Flux: Not Permitted N/A
* Consumable Inserts conforming SFA5.30 Class 3, Classification IN317
may also be used.
Welding Procedure Specification (WPS)
Joints (QW-402)
Joint Design: Single V, U or J shown on the other side and repairs, build-up
Backing: Optional for GTAW, Required for SMAW Backing or Retainer type: Non
Member Company Name:
WPS Number 1/8-32-1 (clad pipe) Revision 1 Date issued: 11-13-0
Welding Process: Manual GTAW and SMAW Supporting PQRs: 040
Preheat (QW-406)
Minimum metal temp.: 50° F
Interpass Temp.(Max): 350° F
Preheat Maintenance: None.
Gas (QW-408)
Shielding Gas: Argon, 30 to 40 CFH
Backing Gas: Argon, 15 to 40 CFH
Trailing Shield: None
Positions (QW-405)
Positions permitted: All
Progression when in Vertical: Uphill
Postweld Heat Treatment (QW-407)
Temperature: None
Min. Holding Time: N/A
Weld Electrode or Filler Current Travel Speed* Other
Layer Process Class Diameter Type Polarity Volts Current (a) (ipm)
Root GTAW ER317L 3/32, 1/8 DC EN (str.) N/A 70 to 115 1 to 2 Higher amperage
Fill GTAW ER317L 1/8, 5/32 DC EN (str.) N/A 100 to160 2 to 4 permitted when
insert is used
Fill SMAW E317L-15 3/32 DC EP (rev.) N/A 70 to 90 2 to 4
SMAW or 1/8 DC EP (rev.) N/A 80 to 110 2 to 4 *Values are
SMAW E317L-16 5/32 DC EP (rev.) N/A 120 to 160 2 to 6 recommended on
Technique (QW-410)
Tungsten Size and Type: 3/32, 1/8 EWTh-2,EWLa or EWCe Initial Cleaning: Remove grease or oil with solvent.
Shielding Gas Cup Size: #4 (1/4” ID) to #12 (3/4” ID) Remove cutting oxide by grinding.Single or Multiple Pass per Side: Multiple Interpass Cleaning: Remove slag with slag hammer, grinder or
Single or Multiple electrodes: Single wire brush.
Contact-tube-to-work distance (stickout): N/A Peening: Not permitted
Backgouging: Grinding or carbon arc followed by grinding Other: Keep weld beads slightly convex to avoid cracking.
Repair Method: Grinding. Backwelding is permitted.
Stringer or Weave Bead: Either, but keep any weave small.
The undersigned contractor, a member of the National Certified Pipe welding Bureau, hereby adopts this jointly developed procedure as its
Welding Procedure Specification (WPS) and certifies that this procedure has been qualified as shown on the attached Procedure Qualification
Records (PQRs).
Company:
B : Date: NCPWB W-482/5-02 WPS 1/8-32-
Electrical Characteristics (QW-409) and Related Matters
8/13/2019 Welding Procedure for pipes
http://slidepdf.com/reader/full/welding-procedure-for-pipes 4/5
Joint Designs for Joining Internally Clad Piping by WeldingPreferred Weld End Preparation and Fit-up
30 to 45° Typ
R=1/8 min
3/32 to1/8”1/16 in max 1/16 to 3/32”
33 to 45° Typ
R=1/8 min
0 to 1/32”clearance1/16 in max
P-1 Pipe
Wall
P-8
Cladding
1/16 to 3/32”
Open Root Adding ER317L
Filler MetalClass 3 Consumable Insert meeting
IN317L analysis
Secondary Weld End Preparation and Fit-up
Third Possible Weld End Preparation and Fit-up
3/32 in Max
30 to 45°
0 to 1/32”clearance
P-1 Pipe
Wall
P-8
Cladding
Class 3 Consumable Insert meeting
IN317L analysis
3/32 to 1/8”
1/16 in max
30 to 45°
0 to 1/16 in
3/16”Minimum
P-1 Pipe
Wall
P-8Cladding
Tack
Step 2: fit up using blocks that are tack welded
to groove faces to hold root spacing
Step 3: Build up root faces using GTAW Step 4: Weld Root Pass
8/13/2019 Welding Procedure for pipes
http://slidepdf.com/reader/full/welding-procedure-for-pipes 5/5
Weld Electrode or Filler Current Travel Speed Other
Layer Process Class Dia (in) Type Polarity Volts Current (a) (ipm)
Root GTAW ER317L 1/8 DC EN (str.) N/A 85 1.5 28,900 kJ/in
Fill GTAW ER317L 1/8 DC EN (str.) N/A 120 2
Fill GTAW ER317L 5/32 DC EN (str.) N/A 140 2
Fill SMAW E317L-16 1/8 DC EP (rev.) N/A 76 2.5
Fill SMAW E317L-16 1/8 DC EP (rev.) N/A 89 to 101 1.75 to 2
Procedure Qualification RecordIdentification of WPS followed during welding of test coupon: 1/8-32-2
Welding Process(es) used: GTAW followed by SMAW, Manual Date coupon was welded: 3-1-03
Base Metal Specification: SA-516-70 clad w/SA240 Type 317L to Base Metal Specification: Same
P-Number: 1, 8 Group No: 2, 1 to P-Number: 1, 8 Group No: 2,1 Plate/Pipe Diameter: NPS 10 Sch 60
Base Metal Thickness(in.): 0.5 + 0.05 clad Joint Type: Single V-groove F-Number: 6/5
Filler metal specification: SFA 5.9 / SFA 5.4 AWS Classification: ER317L/E317L-16
A-Number: 8/8 Weld Deposit Thickness(es)(in.): 0.2/0.35 Maximum Pass Thickness: 5/32, 3/16Filler metal size (in): 1/8, 5/32 GTA/ 3/32, 1/8 GTA Supplementary filler metal: N/A
Preheat temperature (ºF): 75 Interpass temperature (ºF) 350 Welding position/progression: 5G Uphill
Current Type and polarity: DCEN/DCEP Travel speed (ipm): see below
Shielding gas composition, CFH: Argon, 35 Backing gas composition, CFH: Argon, 45 CFH
Tungsten size/type: 1/8”, EWTh-2 GMAW transfer mode: N/A
Postweld Heat treatment (ºF): None Postweld heat treatment time (hr.): N/A
Stringer/Weave bead: Both Oscillation: N/A
Single/Multi-pass: Multiple Single/Multi-electrode: Single
Other:
Reduced Section Tensile Tests X Rectangular Turned Full Section
Bend Tests Transverse Face and Root x Side Longitudinal Face and Root
Specimen Width/Dia (in.) Thickness (in) Area (sq in.) Ultimate load (lb.) Ultimate Stress (psi) Failure Location
1 0.542 0.4989 0.270 22,762 84,300 Base Metal, Ductile
2 0.519 0.5327 0.276 23,164 83,900 Base Metal, Ductile
Type Results Type Results
Side Acceptable Side Acceptable
Side Acceptable Side Acceptable
Toughness Tests Charpy Specimen Size Test TemperatureSpecimen Notch Location Ft. Lb. Lateral Expansion (mils) Percent Shear Drop Weight Break No Break
1
2
3Weld deposit analysis: SMAW Weld, C:0.06, Mn:0.96, Si:0.38, Ni:22.79, Cr: 14.89, Mo:3.67, Cu:0.24, Nb:0.76, Ti:0.05
Other tests: HRB: CS BM 81, 81, 82. CS HAZ: 86, 85, 84. SS BM: 81, 80, 84. SS HAZ: 85, 85, 90. WM: 91, 90, 90, 90, 91, 94
Welder’s name: Dave Hintz Stamp: H2294 Welding Witnessed by: Paul Robertson, J. H. Robertson Co
Tests conducted by: Kish, C. J. Latropulos, PE, #38489 Laboratory test number: 1032019/20098
We hereby certify that the statements in this record are correct and that the test welds were prepared, welded and tested in accordanc
with the requirements of Section IX of the ASME Code.
National Certified Company:
Pipe Welding Bureau
Chairman, Technical Committee PQR Number 04016
By: Date: