122
THEORY OF METAL CUTTING Thermal aspects of Machining, Tool materials, Tool wear Cutting fluids and Machinability. ME 010 803 PRODUCTION ENGINEERING Module II

Theory of metal cutting-module II

Embed Size (px)

DESCRIPTION

As per syllabus of MG university. Production Engineering, 8th Semester B.Tech Mechanical Engineering

Citation preview

Page 1: Theory of metal cutting-module II

THEORY OF METAL CUTTING

Thermal aspects of Machining,Tool materials, Tool wear

Cutting fluids and Machinability.

ME 010 803 PRODUCTION ENGINEERINGModule II

Page 2: Theory of metal cutting-module II

Cutting TemperaturesOf the total energy consumed in machining, nearly all of it is converted into heat. The heat generated can cause temperatures to be as high as 6000C at tool chip interface.

Cutting temperature has a controlling influence on the rate of tool wear and friction between tool and chip.

Elastic deformation- Energy required for the operation is stored in the material as strain energy and no heat is generated.Plastic deformation – Most of the energy used is converted as heat.

Page 3: Theory of metal cutting-module II

Cutting TemperaturesCutting temperatures are important because high temperatures,

1. Reduce tool life.

2. Produce hot chips that pose safety hazards to the machine operator.

3. Can cause inaccuracies in work part dimensions due to thermal expansion of work piece material.

Page 4: Theory of metal cutting-module II

Effect of cutting temperature

The effect of cutting temperature, particularly when it is high is mostly detrimental to both the tool and the job.

The major portion of the heat is taken away by the chips. But it does not matter because chips are thrown out.

So attempts should be made such that the chips take away more and more amount of heat leaving small amount of heat to harm the tool and the job.

Page 5: Theory of metal cutting-module II

Effect of cutting temperature on tool

The possible detrimental effects of the high cutting temperature on cutting tool (edge) are

Rapid tool wear which reduces tool life

plastic deformation of the cutting edges if the tool material is not enough hot-hard and hot-strong

thermal flaking and fracturing of the cutting edges due to thermal shocks.

Built up Edge formation.

Page 6: Theory of metal cutting-module II

Effect of cutting temperature on Job

The possible detrimental effects of the high cutting temperature on machined job are:

Dimensional inaccuracy of the job due to thermal distortion and expansion-contraction during and after machining

surface damage by oxidation, rapid corrosion, burning etc.

induction of tensile residual stresses and micro cracks at the surface / subsurface.

Page 7: Theory of metal cutting-module II

Effect of Cutting TemperatureHowever, often the high cutting temperature helps in reducing the magnitude of the cutting forces and cutting power consumption to some extent by softening or reducing the shear strength, τs of the work material ahead the cutting edge.

To attain or enhance such benefit the work material ahead the cutting zone is often additionally heated externally. This technique is known as Hot Machining and is beneficially applicable for the work materials which are very hard and hardenable like high manganese steel, Hadfield steel, Ni-hard, Nimonic etc.

Page 8: Theory of metal cutting-module II

Factors Affecting Temperature

Page 9: Theory of metal cutting-module II

Sources and Causes of heat generation in Machining

During machining, heat is generated at the cutting point from three sources, as indicated in Fig.

Those sources and causes of development of cutting temperature are: Primary shear zone (1) where the major part of the energy

is converted into heat. Secondary deformation zone (2) at the chip – tool

interface where further heat is generated due to rubbing and / or shear.

At the worn out flanks (3) due to rubbing between the tool and the finished surfaces.

Page 10: Theory of metal cutting-module II

Sources of heat generation in Machining

Page 11: Theory of metal cutting-module II

Thermal Aspects of MachiningThe heat generated is shared by the chip, cutting tool and the blank.

The apportionment of sharing the heat depends upon the

configuration, size and thermal conductivity of the tool – work

material and the cutting condition.

The following figure visualizes that maximum amount of heat is

carried away by the flowing chip.

From 10 to 20% of the total heat goes into the tool and some heat is

absorbed in the blank.

With the increase in cutting velocity, the chip shares heat

increasingly.

Page 12: Theory of metal cutting-module II

Thermal Aspects of Machining

Page 13: Theory of metal cutting-module II

Temperature distribution in Metal Cutting

Fig. shows temperature distribution in work piece and chip during orthogonal cutting (obtained from an infrared photograph, for free-cutting mild steel where cutting speed is 0.38m/s, the width of cut is 6.35mm, the normal rake is 300, and work piece temperature is 6110C)

Page 14: Theory of metal cutting-module II

Temperature distribution in Metal Cutting

Page 15: Theory of metal cutting-module II

Analytical methods to compute Cutting Temperatures

Cook’s Method

Where,

δT = Mean temperature rise at tool chip interface, C0

U = Specific Energy in the operation, N-m/mm3

V = Cutting Speed, m/st0 = Chip thickness before the cut, m

ρC = Volumetric Specific heat of work material, J/mm3-C0

K = Thermal diffusivity of the work material, m2/s

0.333

04.0

K

Vt

C

UT

Page 16: Theory of metal cutting-module II

Measurement of tool-chip interface temperature

Page 17: Theory of metal cutting-module II

Tool work Thermocouple Technique

In a thermocouple two dissimilar but electrically conductive metals are connected at two junctions.

Whenever one of the junctions is heated, the difference in temperature at the hot and cold junctions produce a proportional current which is detected and measured by a milli-voltmeter.

In machining like turning, the tool and the job constitute the two dissimilar metals and the cutting zone functions as the hot junction.

Then the average cutting temperature is evaluated from the mV after thorough calibration for establishing the exact relation between mV and the cutting temperature.

Page 18: Theory of metal cutting-module II

Tool work thermocouple technique

Page 19: Theory of metal cutting-module II

Embedded thermocouple technique In operations like milling, grinding etc. where the previous methods are not applicable, embedded thermocouple can serve the purpose. Fig. shows the principle.

The standard thermocouple monitors the job temperature at a certain depth, hi

from the cutting zone. The temperature recorded in oscilloscope or strip chart recorder becomes maximum when the thermocouple bead comes nearest (slightly offset) to the grinding zone.

With the progress of grinding the depth, hi gradually decreases after each

grinding pass and the value of temperature, θm also rises as has been

indicated in Fig.

For getting the temperature exactly at the surface i.e., grinding zone, h i

has to be zero, which is not possible. So the θm vs hi

curve has to be extrapolated up to hi = 0 to get the actual grinding zone temperature. Log – log plot helps such extrapolation more easily and accurately.

Page 20: Theory of metal cutting-module II

Embedded thermocouple technique

Page 21: Theory of metal cutting-module II

Infra-red photographic technique

This modern and powerful method is based on taking infra-red photograph of the hot surfaces of the tool, chip, and/or job and get temperature distribution at those surfaces.

Proper calibration is to be done before that. This way the temperature profiles can be recorded as indicated in Fig.

The fringe pattern readily changes with the change in any machining parameter which affect cutting temperature.

Page 22: Theory of metal cutting-module II

Infra-red photographic technique

Page 23: Theory of metal cutting-module II

Tool wear and failureThe usefulness of tool cutting edge is lost through

Wear

Breakage

Chipping

Deformation

Tool failure implies that the tool has reached a point beyond which it will not function satisfactorily until it is re-sharpened.

Page 24: Theory of metal cutting-module II

Three Modes of Tool FailureFracture failure

When the Cutting force at tool point becomes excessive, it leads to failure by brittle fracture.

Temperature failure Cutting temperature is too high for the tool material, which makes the tool point to soften, and leads to plastic deformation along with a loss of sharp edge.

Gradual wear Gradual wearing of the cutting edge causes loss of tool shape, reduction in cutting efficiency and finally tool failure.

Page 25: Theory of metal cutting-module II

Preferred Mode of Tool Failure: Gradual Wear

Fracture and temperature failures are premature failures

Gradual wear is preferred because it leads to the longest possible use of the tool

Gradual wear occurs at two locations on a tool:

Crater wear – occurs on top rake face

Flank wear – occurs on flank (side of tool)

Page 26: Theory of metal cutting-module II

Figure: Diagram of worn cutting tool, showing the principal locations and types of wear that occur

Page 27: Theory of metal cutting-module II

Crater wearIt consists of a concave section on the tool face formed by the action of the chip sliding on the surface.

Crater wear affects the mechanics of the process increasing the actual rake angle of the cutting tool and consequently, making cutting easier.

At the same time, the crater wear weakens the tool wedge and increases the possibility for tool breakage.

In general, crater wear is of a relatively small concern.

Page 28: Theory of metal cutting-module II
Page 29: Theory of metal cutting-module II

Flank wear It occurs on the tool flank as a result of friction between the

machined surface of the work piece and the tool flank.

Flank wear appears in the form of so-called wear land and is measured by the width of this wear land, VB, Flank wear affects to the great extend the mechanics of cutting.

Cutting forces increase significantly with flank wear.

If the amount of flank wear exceeds some critical value i.e. (VB > 0.5~0.6 mm), the excessive cutting force may cause tool failure.

Page 30: Theory of metal cutting-module II

Corner Wear It occurs on the tool corner.

Can be considered as a part of the wear land and respectively flank wear since there is no distinguished boundary between the corner wear and flank wear land.

We consider corner wear as a separate wear type because of its importance for the precision of machining.

Corner wear actually shortens the cutting tool thus increasing gradually the dimension of machined surface and introducing a significant dimensional error in machining, which can reach values of about 0.03~0.05 mm.

Page 31: Theory of metal cutting-module II
Page 32: Theory of metal cutting-module II
Page 33: Theory of metal cutting-module II

Figure :

(a)Crater wear, and

(b)flank wear on a cemented carbide tool,

as seen through a toolmaker's microscope

Page 34: Theory of metal cutting-module II

Tool Wear: Mechanisms Adhesion wear:

Fragments of the work-piece get welded to the tool surface at high temperatures; eventually, they break off, tearing small parts of the tool with them.

Abrasion:

Hard particles, microscopic variations on the bottom surface of the chips rub against the tool surface and break away a fraction of tool with them.

Diffusion wear:

At high temperatures, atoms from tool diffuse across to the chip; the rate of diffusion increases exponentially with temperature; this reduces the fracture strength of the crystals.

Page 35: Theory of metal cutting-module II

Figure: Tool wear as a function of cutting time Flank wear (FW) is used here as the measure of tool wear

Crater wear follows a similar growth curve

Tool Wear vs. Time

Page 36: Theory of metal cutting-module II

Factors affecting Tool life Tool material

Hardness

Work material

Surface roughness of work piece

Profile of cutting tool

Type of machining operation

Cutting speed, feed and depth of cut

Cutting temperature

Page 37: Theory of metal cutting-module II

Tool life Criteria

Actual cutting time to failure.

Length of work cut to failure.

Volume of metal removed to failure.

Cutting speed for a given time to failure.

Number of components produced.

Page 38: Theory of metal cutting-module II

Figure: Effect of cutting speed on tool flank wear (FW) for three cutting speeds, using a tool life criterion of 0.50 mm flank wear

Effect of Cutting Speed

Page 39: Theory of metal cutting-module II

Figure: Natural log‑log plot of cutting speed vs tool life

Page 40: Theory of metal cutting-module II

Tool Life Tool wear is a time dependent process. As cutting

proceeds, the amount of tool wear increases gradually.

Tool wear must not be allowed to go beyond a certain limit in order to avoid tool failure.

Tool life is defined as the time interval for which tool works satisfactorily between two successive grinding or re-sharpening of the tool.

Page 41: Theory of metal cutting-module II

Taylor Tool Life EquationThis relationship is credited to F. W. Taylor (~1900)

CvT n

Where, v = cutting speed;

T = tool life; and

n and C are parameters that depend on feed, depth of cut, work material, tooling material, and the tool life criterion used

n is the slope of the plot

C is the intercept on the speed axis

Page 42: Theory of metal cutting-module II

Tool Life vs. Cutting Speed

As cutting speed is increased, wear rate increases, so the same wear criterion is reached in less time, i.e., tool life decreases with cutting speed

Page 43: Theory of metal cutting-module II

Typical Values of n and C in Taylor’s Tool Life Equation

Tool material n C (m/min) C (ft/min)

High speed steel:

Non-steel work 0.125 120 350

Steel work 0.125 70 200

Cemented carbide

Non-steel work 0.25 900 2700

Steel work 0.25 500 1500

Ceramic

Steel work 0.6 3000 10,000

Page 44: Theory of metal cutting-module II

Tool life

Volume of metal removed per minute Vm

Vm = . . . 𝜋𝐷 𝑡 𝑓 𝑁 𝑚𝑚3/ in 𝑚

D = dia of workpiece, mm

t = depth of cut, mm

f = feed, mm/rev

N = RPM

Page 45: Theory of metal cutting-module II

Tool Life If T be the time for tool failure in mins, The total volume removed up to Tool Failure

= . . . . 𝝅𝑫 𝒕 𝒇 𝑵 𝑻𝒎𝒎𝟑

Cutting Speed,

V = DN/ 000 m/min 𝝅 𝟏Volume of material removed up to tool failure

= 000 V. . . 𝟏 𝒇 𝑻 𝒕 𝒎𝒎 𝟑

Page 46: Theory of metal cutting-module II

Tool Near End of Life Changes in sound emitted from operation.

Chips become ribbon-like, stringy, and difficult to dispose off.

Degradation of surface finish.

Increased power required to cut.

Visual inspection of the cutting edge with magnifying optics can determine if tool should be replaced.

Page 47: Theory of metal cutting-module II

Tool life is measured by: Visual inspection of tool edge Tool breaks Fingernail test Changes in cutting sounds Chips become ribbony, stringy Surface finish degrades Computer interface says

- power consumption up

- cumulative cutting time reaches certain level

- cumulative number of pieces reaches certain value

Tool life is measured by: Visual inspection of tool edge Tool breaks Fingernail test Changes in cutting sounds Chips become ribbony, stringy Surface finish degrades Computer interface says

- power consumption up

- cumulative cutting time reaches certain level

- cumulative number of pieces reaches certain value

Operator’s Tool life

Page 48: Theory of metal cutting-module II

Wear Control The rate of tool wear strongly depends on the cutting

temperature, therefore, any measures which could be applied to reduce the cutting temperature would reduce the tool wear as well.

The figure shows the process parameters that influence the rate of tool wear:

Additional measures to reduce the tool wear include the application of advanced cutting tool materials, such as coated carbides, ceramics, etc..

Page 49: Theory of metal cutting-module II

Wear Control

Page 50: Theory of metal cutting-module II

Cutting Tool Technology It has two principal aspects:

1. Tool material

Developing materials that can withstand the forces, temperatures and wearing in machining process.

2. Tool geometry

Optimizing the geometry of the cutting tool for the tool material and for a given operation.

Page 51: Theory of metal cutting-module II

The cutting tool materials must possess a number of important properties to avoid excessive wear, fracture failure and high temperatures in cutting.

The following characteristics are essential for cutting materials to withstand the heavy conditions of the cutting process and to produce high quality and economical parts:

Tool failure modes identify the important properties that a tool material should possess:

Toughness ‑ to avoid fracture failure.

Hot hardness ‑ ability to retain hardness at high temperatures.

Wear resistance ‑ hardness is the most important property to resist abrasive wear.

CUTTING TOOL MATERIALS

Page 52: Theory of metal cutting-module II

CUTTING TOOL MATERIALS hardness at elevated temperatures (so-called hot hardness) so

that hardness and strength of the tool edge are maintained in high cutting temperatures.

Toughness: ability of the material to absorb energy without failing. Cutting is often accompanied by impact forces especially if cutting is interrupted, and cutting tool may fail very soon if it is not strong enough.

wear resistance: although there is a strong correlation between hot hardness and wear resistance, latter depends on more than just hot hardness. Other important characteristics include surface finish on the tool, chemical inertness of the tool material with respect to the work material, and thermal conductivity of the tool material, which affects the maximum value of the cutting temperature at tool-chip interface.

Page 53: Theory of metal cutting-module II

Fig: Typical hot hardness relationships for selected tool materials.

Plain carbon steel shows a rapid loss of hardness as temperature increases.High speed steel is substantially better, while cemented carbides and ceramics are significantly harder at elevated temperatures.

Page 54: Theory of metal cutting-module II

Carbon Steels It is the oldest of tool material. It is inexpensive, easily

shaped, sharpened.

The carbon content is 0.6~1.5% with small quantities of silicon, chromium, manganese, and vanadium to refine grain size.

This material has low wear resistance and low hot hardness. Maximum hardness is about HRC 62.

Used for drills taps, broaches, reamers.

Limited to hand tools and low cutting speed operation. (Red hardness temp.: 200° C)

The use of these materials now is very limited.

Page 55: Theory of metal cutting-module II

High Speed Steel (HSS) First produced in 1900s. They are highly alloyed with

vanadium, cobalt, molybdenum, tungsten and chromium added to increase hot hardness and wear resistance.

Can be hardened to various depths by appropriate heat treating up to cold hardness in the range of HRC 63-65.

The cobalt component give the material a hot hardness value much greater than carbon steels.(Red hardness temp.: 6500 C)

The high toughness and good wear resistance make HSS suitable for all type of cutting tools with complex shapes for relatively low to medium cutting speeds.

Page 56: Theory of metal cutting-module II

High Speed Steel (HSS) Highly alloyed tool steel capable of maintaining hardness

at elevated temperatures better than high carbon and low alloy steels.

One of the most important cutting tool materials

Especially suited to applications involving complicated tool geometries, such as The most widely used tool material today for taps, drills, reamers, gear tools, end cutters, slitting, broaches, etc.

Two basic types

1. Tungsten‑type, designated T‑ grades

2. Molybdenum‑type, designated M‑grades

Page 57: Theory of metal cutting-module II

High Speed Steel CompositionTwo basic types of HSS

M-series (6-6-4-2): Contains 6% molybdenum, 6% tungsten, 4% chromium,

2% vanadium & cobalt Higher, abrasion resistance H.S.S. are majorly made of M-series

T-series (18-4-1): Contains 18 % tungsten, 4% chromium, 1% vanadium

& cobalt undergoes less distortion during heat treating

Page 58: Theory of metal cutting-module II

Cemented Carbides Introduced in the 1930s. These are the most important

tool materials today because of their high hot hardness and wear resistance.

There may be other carbides in the mixture, such as titanium carbide (TiC) and/or tantalum carbide (TaC) in addition to WC.

The main disadvantage of cemented carbides is their low toughness.

Page 59: Theory of metal cutting-module II

Cemented Carbides – General Properties

High compressive strength, but low to moderate tensile strength

High hardness (90 to 95 HRA)

Good hot hardness

Good wear resistance

High thermal conductivity

High elastic modulus ‑ 600 x 103 MPa (90 x 106 lb/in2)

Toughness lower than high speed steel

Page 60: Theory of metal cutting-module II

This hard tool material is produced by a powder metallurgy technique, sintering grains of tungsten carbide (WC) in a cobalt (Co) matrix (as the binder, it provides toughness).

Particles 1-5 μm in size are pressed & sintered to desired shape in a H2 atmosphere furnace at 15500 C.

Amount of cobalt present affects properties of carbide tools. As cobalt content increases – strength, hardness & wear resistance increases.

Cemented Carbides

Page 61: Theory of metal cutting-module II

Cemented Carbides

Page 62: Theory of metal cutting-module II

Insert AttachmentIn spite of more traditional tool materials, cemented carbides are available as

inserts produced by powder metallurgy process.Inserts are available in various shapes, and are usually mechanically attached

by means of clamps to the tool holder, or brazed to the tool holder. The clamping is preferred because after an cutting edge gets worn, the insert

is indexed (rotated in the holder) for another cutting edge. When all cutting edges are worn, the insert is thrown away. The indexable

carbide inserts are never reground.If the carbide insert is brazed to the tool holder, indexing is not available, and

after reaching the wear criterion, the carbide insert is re-sharpened on a tool grinder.

Page 63: Theory of metal cutting-module II

Types of Cemented Carbides

Two basic types:

1. Non‑steel cutting grades - only WC‑Co

2. Steel cutting grades - TiC & TaC added to WC‑Co

Page 64: Theory of metal cutting-module II

Non‑Steel Cutting Carbide Grades

• Used for nonferrous metals and gray cast iron

• Properties determined by grain size and cobalt content

– As grain size increases, hardness and hot hardness decrease, but toughness increases.

– As cobalt content increases, toughness improves at the expense of hardness and wear resistance.

Page 65: Theory of metal cutting-module II

Steel Cutting Carbide Grades

Used for low carbon, stainless, and other alloy steels

– For these grades, TiC and/or TaC are substituted for some of the WC.

– This composition increases crater wear resistance for steel cutting, but adversely affects flank wear resistance for non‑steel cutting applications.

Page 66: Theory of metal cutting-module II

Coated WCOne advance in cutting tool materials involves the application of a very thin coating (~ 10 μm) to a K-grade substrate, which is the toughest of all carbide grades.

Coating may consists of one or more thin layers of wear-resistant material, such as titanium carbide (TiC), titanium nitride (TiN), aluminum oxide (Al2O3), and/or other, more advanced materials.

Coating allows to increase significantly the cutting speed for the same tool life.

Structure of a multi-layer coated carbide insert

Page 67: Theory of metal cutting-module II

Coated Carbides Cemented carbide insert coated with one or more thin layers of wear resistant materials, such as TiC, TiN, and/orAl2O3

Coating is applied by chemical vapor deposition or physical vapor deposition.

Coating thickness = 2.5 ‑ 13 m (0.0001 to 0.0005 in)

Applications: cast irons and steels in turning and milling operations.

Best applied at high speeds where dynamic force and thermal shock are minimal.

Page 68: Theory of metal cutting-module II

Ceramics Primarily fine‑grained Al2O3, pressed and sintered at high pressures and temperatures into insert form with no binder.

• Applications: high speed turning of cast iron and steel

• Not recommended for heavy interrupted cuts (e.g. rough milling) due to low toughness

• There is no occurrence of built-up edge, and coolants are not required.

• Al2O3 also widely used as an abrasive in grinding.

Page 69: Theory of metal cutting-module II

Ceramics Two types are available:

White or cold-pressed ceramics, which consists of only Al2O3 cold pressed into inserts and sintered at high temperature.

Black or hot-pressed ceramics, commonly known as cermet (from ceramics & metal). This material consists of 70% Al2O3 and 30% TiC.

Both materials have very high wear resistance but low toughness, therefore they are suitable only for continuous operations such as finishing turning of cast iron and steel at very high speeds.

Page 70: Theory of metal cutting-module II

Cermets Combinations of TiC, TiN, and titanium carbonitride (TiCN), with nickel and/or molybdenum as binders.

Some chemistries are more complex.

Applications:

high speed finishing and semi-finishing of steels, stainless steels and cast irons.

– Higher speeds and lower feeds than steel‑cutting carbide grades

– Better finish achieved, often eliminating need for grinding.

Page 71: Theory of metal cutting-module II

Diamond• Diamond is the hardest substance ever known of all

materials.

• Low friction, high wear resistance.

• Ability to maintain sharp cutting edge.

• Use is limited because it gets converted into graphite at high temperature (700 °C). Graphite diffuses into iron and make it unsuitable for machining steels.

• It is used as a coating material in its polycrystalline form, or as a single- crystal diamond tool for special applications, such as mirror finishing of non-ferrous materials.

Page 72: Theory of metal cutting-module II

Synthetic Diamonds Sintered polycrystalline diamond (SPD) - fabricated by sintering very fine grained diamond crystals under high temperatures and pressures into desired shape with little or no binder.

Usually applied as coating (0.5 mm thick) on WC-Co insert

Applications: high speed machining of nonferrous metals and abrasive nonmetals such as fiberglass, graphite, and wood.

- Not for steel cutting

Page 73: Theory of metal cutting-module II

Cubic Boron Nitride Next to diamond, cubic boron nitride (CBN) is hardest

material known. Retain hardness up to 1000°C.

By bonding 0.5 mm thick polycrystalline CBN onto a carbide substrate through sintering under pressure.

CBN is used mainly as coating material because it is very brittle.

In spite of diamond, CBN is suitable for cutting ferrous materials.

Applications: machining steel and nickel‑based alloys.

Page 74: Theory of metal cutting-module II

SPD and CBN tools are expensive.

Made by bonding (0.5-1.0 mm) Layer of poly crystalline cubic boron nitride to a carbide substrate by sintering under Pressure.

While carbide provides shock resistance CBN layer provides high resistance and cutting edge strength.

Cubic boron nitride tools are made in small sizes without substrate.

Cubic Boron Nitride

Page 75: Theory of metal cutting-module II

Lubricants – purpose is to reduce friction… usually oil based

Coolants – purpose is to transport heat… usually water based

Both lose their effectiveness at higher cutting speeds!

Lubricants – purpose is to reduce friction… usually oil based

Coolants – purpose is to transport heat… usually water based

Both lose their effectiveness at higher cutting speeds!

Cutting Fluids

Page 76: Theory of metal cutting-module II

Dry Machining• No cutting fluid is used

• Avoids problems of cutting fluid contamination, disposal, and filtration

• Problems with dry machining:

– Overheating of the tool

– Operating at lower cutting speeds and production rates to prolong tool life

– Absence of chip removal benefits of cutting fluids in grinding and milling

Page 77: Theory of metal cutting-module II

77

Cutting Fluids• Essential in metal-cutting operations to reduce heat and

friction

• Centuries ago, water used on grindstones

• 100 years ago, tallow used (did not cool)

• Lard oils came later but turned rancid

• Early 20th century saw soap added to water

• Soluble oils came in 1936

• Chemical cutting fluids introduced in 1944

Page 78: Theory of metal cutting-module II

Cutting FluidsAny liquid or gas applied directly to machining operation to improve cutting performance

Two main problems addressed by cutting fluids:

1. Heat generation at shear zone and friction zone

2. Friction at the tool ‑ chip and tool ‑ work interfaces

Other functions and benefits:

– Wash away chips (e.g., grinding and milling)

– Reduce temperature of work part for easier handling

– Improve dimensional stability of work part

Page 79: Theory of metal cutting-module II

79

Heat Generated During Machining• Heat finds its way into one of three places–Work piece, tool and chips

Too much, workwill expandToo much, cutting edge will

break down rapidly, reducing tool life

Act as disposable heat sink

Page 80: Theory of metal cutting-module II

80

Heat Dissipation

• Ideally most heat taken off in chips

• Indicated by change in chip colour as heat causes chips to oxidize.

• Cutting fluids assist taking away heat

– Can dissipate at least 50% of heat created during machining.

Page 81: Theory of metal cutting-module II

Characteristics of a Good Cutting Fluid

Page 82: Theory of metal cutting-module II

82

Characteristics of a Good Cutting Fluid

1. Good cooling capacity

2. Good lubricating qualities

3. Resistance to rancidity

4. Relatively low viscosity

5. Stability (long life)

6. Rust resistance

7. Nontoxic

8. Transparent

9. Non inflammable

Page 83: Theory of metal cutting-module II

83

Economic Advantages to Using Cutting Fluids

Reduction of tool costs.– Reduce tool wear, tools last longer

Increased speed of production.– Reduce heat and friction so higher cutting speeds

Reduction of labor costs.– Tools last longer and require less regrinding, less

downtime, reducing cost per part

Reduction of power costs.– Friction reduced so less power required by machining

Page 84: Theory of metal cutting-module II

84

Functions of a Cutting Fluid

Prime functions

– Provide cooling

– Provide lubrication

Other functions

– Prolong cutting-tool life

– Provide rust control

– Resist rancidity

Page 85: Theory of metal cutting-module II

85

Functions of a Cutting Fluid: Cooling

• Most effective at high cutting speeds where heat generation and high temperatures are problems.

• Most effective on tool materials that are most susceptible to temperature failures. (e.g., HSS)

• Two sources of heat during cutting action

– Plastic deformation of metal• Occurs immediately ahead of cutting tool

• Accounts for 2/3 to 3/4 of heat

– Friction from chip sliding along cutting-tool face.

Page 86: Theory of metal cutting-module II

86

Functions of a Cutting Fluid: Cooling

• Water used as base in coolant ‑ type cutting fluids.

• Water most effective for reducing heat by will promote oxidation (rust).

• Heat has definite bearing on cutting-tool wear

– Small reduction will greatly extend tool life

• Decrease the temperature at the chip-tool interface by 50 degrees F, and it will increase tool life by up to 5 times.

Page 87: Theory of metal cutting-module II

87

Functions of a Cutting Fluid: Lubrication

• Usually oil based fluids and are most effective at lower cutting speeds.

• Also reduces temperature in the operation.

• Reduces friction between chip and tool face

– Shear plane becomes shorter

– i.e., the area where plastic deformation occurs is smaller

• Extreme-pressure lubricants reduce amount of heat produced by friction.

• EP chemicals of synthetic fluids combine chemically with sheared metal of chip to form solid compounds (allows chip to slide)

Page 88: Theory of metal cutting-module II

88

Cutting fluid reduces friction and produces a shorter shear plane.

Page 89: Theory of metal cutting-module II

89

Cutting-Tool Life

• Heat and friction are prime causes of cutting-tool breakdown

• Reduce temperature by as little as 500F, life of cutting tool increases fivefold

• Built-up edge

– Pieces of metal weld themselves to tool face

– Becomes large and flat along tool face, effective rake angle of cutting tool decreased

Page 90: Theory of metal cutting-module II

90

Built-up Edge

Built-up edge keeps breaking off and re-forming and result is poor surface finish, excessive flank wear, and cratering of tool face.

Page 91: Theory of metal cutting-module II

91

Cutting Fluid's Effect on Cutting Tool Action

1. Lowers heat created by plastic deformation of metal

2. Friction at chip-tool interface decreased

3. Less power is required for machining because of reduced friction

4. Prevents built-up edge from forming

5. Surface finish of work greatly improved

Page 92: Theory of metal cutting-module II

92

Rust Control

• Water is the best and most economical coolant

– Causes parts to rust

• Rust is oxidized iron

• Chemical cutting fluids contain rust inhibitors

Page 93: Theory of metal cutting-module II

93

Rancidity Control

Rancidity caused by bacteria and other microscopic organisms, growing and eventually causing bad odours to form.

Most cutting fluids contain bactericides that control growth of bacteria and make fluids more resistant to rancidity.

Page 94: Theory of metal cutting-module II

94

Application of Cutting Fluids

• Cutting-tool life and machining operations influenced by way cutting fluid applied

• Copious stream under low pressure so work and tool well covered

– Inside diameter of supply nozzle ¾ width of cutting tool

– Applied to where chip being formed

Page 95: Theory of metal cutting-module II

95

Refrigerated Air System• Another way to cool chip-tool interface

• Effective, inexpensive and readily available

• Used where dry machining is necessary

• Uses compressed air that enters vortex generation chamber

– Cooled 1000F below incoming air

• Air directed to interface and blow chips away

Page 96: Theory of metal cutting-module II

96

Types of Cutting Fluids

• Most commonly used cutting fluids

– Either aqueous based solutions or cutting oils

• Fall into three categories

– Straight Cutting oils

– Emulsifiable oils or Water Soluble oils

– Chemical (synthetic) cutting fluids

Page 97: Theory of metal cutting-module II

97

Straight Cutting Oils• Derived from petroleum, animal, marine or vegetable

substances and may be used straight or in combination.

• Their main function is lubrication and rust prevention.

• They are chemically stable and lower in cost.

• Usually restricted to light duty machining on metals of high

machinability, such as aluminium, magnesium, brass and

leaded steels.

– Two classifications

» Active

» Inactive

Page 98: Theory of metal cutting-module II

98

Active Cutting Oils

• Those that will darken copper strip immersed for 3 hours at temperature of 2120F

• Dark or transparent

• Better for heavy-duty jobs

• Three categories

– Sulfurized mineral oils

– Sulfochlorinated mineral oils

– Sulfochlorinated fatty oil blends

Page 99: Theory of metal cutting-module II

99

Inactive Cutting Oils• Oils will not darken copper strip immersed in them for 3

hours at 2120F

• Contained sulfur is natural

– Termed inactive because sulfur so firmly attached to oil – very little released

• Four general categories

– Straight mineral oils, fatty oils, fatty and mineral oil blends, sulfurized fatty-mineral oil blend

Page 100: Theory of metal cutting-module II

100

Emulsifiable (Water Soluble) Oils• About 90% of all metal cutting and grinding operations make

use of emulsions due to their high sp. Heat, high thermal conductivity and high heat of vapourisation.

• Mineral oils containing soap like material that makes them soluble in water and causes them to adhere to work piece.

• Emulsifiers break oil into minute particles and keep them separated in water.

– Water blend is in the ratio of 1 part oil to 15~20 parts water (for cutting) and 40 to 60 parts of water (for grinding)

• Good cooling and lubricating qualities.

• Used at high cutting speeds, low cutting pressures.

Page 101: Theory of metal cutting-module II

101

Chemical Cutting Fluids• Also called synthetic fluids

• Introduced about 1945

• Stable, preformed emulsions

– Contain very little oil and mix easily with water

• Extreme-pressure (EP) lubricants added

– React with freshly machined metal under heat and pressure of a cut to form solid lubricant

• Reduce heat of friction and heat caused by plastic deformation of metal

Page 102: Theory of metal cutting-module II

Merits & Demerits of Synthetic Fluids

Page 103: Theory of metal cutting-module II

103

Advantages of Synthetic Fluids Good rust control Resistance to rancidity for long periods of time Reduction of amount of heat generated during cutting due

to Excellent cooling qualities Longer durability than cutting or soluble oils Nonflammable – nonsmoking & Nontoxic ?????? Easy separation from work and chips Quick settling of grit and fine chips so they are not re-

circulated in cooling system No clogging of machine cooling system due to detergent

action of fluid Can leave a residue on parts and tools.

Page 104: Theory of metal cutting-module II

104

Caution Chemical cutting fluids widely accepted

and generally used on ferrous metals.

They are not recommended for use on alloys of magnesium, zinc, cadmium, or lead.

They can mar machine's appearance and dissolve paint on the surface.

Page 105: Theory of metal cutting-module II

105

• Ease or difficulty with which metal can be machined with satisfactory finish at low cost.

• Measured by length of cutting-tool life in minutes or by rate of stock removal in relation to cutting speed employed.

Machinability

Page 106: Theory of metal cutting-module II

MachinabilityMachinability is defined in terms of:

1. Surface finish and surface integrity of machined part

2. Tool life

3. Force and power required

4. The level of difficulty in chip control

Good machinability indicates– good surface finish and surface integrity– a long tool life– and low force and power requirements

Note,

continuous chips should be avoided for good machinability.106

Page 107: Theory of metal cutting-module II

107

Grain Structure• Machinability of metal affected by its microstructure.

• Ductility and shear strength modified greatly by operations such as annealing, normalizing and stress relieving.

• Certain chemical and physical modifications of steel improve Machinability.

– Addition of sulfur, lead, or sodium sulfate

– Cold working, which modifies ductility

Page 108: Theory of metal cutting-module II

Machinability Index

Page 109: Theory of metal cutting-module II

Machinability:Machinability of Nonferrous Metals

• Aluminum– very easy to machine– but softer grades: form BUE poor surface finish⇒– ⇒ recommend high cutting speeds, high rake and relief angles

• Beryllium– requires machining in a controlled environment– this is due to toxicity of fine particles produced in machining

• Cobalt-based alloys– abrasive and work hardening– require sharp, abrasion-resistant tool materials, and low feeds and

speeds

• Copper– can be difficult to machine because of BUE formation

109

Page 110: Theory of metal cutting-module II

Machinability:Machinability of Nonferrous Metals

• Magnesium– very easy to machine, good surface finish, prolonged tool life– Caution: high rate of oxidation and fire danger

• Titanium and its alloys– have very poor thermal conductivity– ⇒ high temp. rise and BUE difficult to machine⇒

• Tungsten– brittle, strong, and very abrasive– ⇒ machinability is low

• Zirconium– Good machinability– Requires cooling cutting fluid (danger of explosion, fire)

110

Page 111: Theory of metal cutting-module II

111

Aluminum• Pure aluminum generally more difficult to machine

than aluminum alloys

– Produces long stringy chips and harder on cutting tool

• Aluminum alloys

– Cut at high speeds, yield good surface finish

– Hardened and tempered alloys easier to machine

– Silicon in alloy makes it difficult to machine

• Chips tear from work (poor surface)

Page 112: Theory of metal cutting-module II

112

Copper• Heavy, soft, reddish-colored metal refined from copper ore

(copper sulfide)

– High electrical and thermal conductivity

– Good corrosion resistance and strength

– Easily welded, brazed or soldered

– Very ductile

• Does not machine well: long chips clog flutes of cutting tool

– Coolant should be used to minimize heat

Page 113: Theory of metal cutting-module II

113

Copper/Beryllium• Heavy, hard, reddish-colored copper metal with Beryllium

added

– High electrical and thermal conductivity.

– Good corrosion resistance and strength.

– Can be welded.

– Somewhat ductile.

– Withstands high temperature.

• Machines well

– Highly abrasive to HSS Tooling.

– Coolant should be used to lubricate and minimize tool wear.

Page 114: Theory of metal cutting-module II

114

Copper-Based Alloys: Brass• Alloy of copper and zinc with good corrosion

resistance, easily formed, machines, and cast.

• Several forms of brass.

– Alpha brasses: up to 36% zinc, suitable for cold working.

– Alpha 1 beta brasses: Contain 54%-62% copper and used in hot working.

• Small amounts of tin or antimony added to minimize pitting effect of salt water.

• Used for water and gas line fittings, tubings, tanks, radiator cores, and rivets.

Page 115: Theory of metal cutting-module II

115

Copper-Based Alloys: Bronze

• Alloys of copper and tin which contain up to 12% of principal alloying element

– Exception: copper-zinc alloys

• Phosphor-bronze

– 90% copper, 10% tin, and very small amount of phosphorus

– High strength, toughness, corrosion resistance

– Used for lock washers, cotter pins, springs and clutch discs

Page 116: Theory of metal cutting-module II

116

Copper-Based Alloys: Bronze

• Silicon-bronze (copper-silicon alloy)

– Contains less than 5% silicon

– Strongest of work-hardenable copper alloys

– Mechanical properties of machine steel and corrosion resistance of copper

– Used for tanks, pressure vessels, and hydraulic pressure lines

Page 117: Theory of metal cutting-module II

117

Copper-Based Alloys: Bronze• Aluminum-bronze (copper-aluminum alloy)

– Contains between 4% and 11% aluminum

– Other elements added

Iron and nickel (both up to 5%) increases strength

Silicon (up to 2%) improves machinability

Manganese promotes soundness in casting

– Good corrosion resistance and strength

– Used for condenser tubes, pressure vessels, nuts and bolts

Page 118: Theory of metal cutting-module II

118

Effects of Temperature and Friction

• Heat created

– Plastic deformation occurring in metal during process of forming chip

– Friction created by chips sliding along cutting-tool face

• Cutting temperature varies with each metal and increases with cutting speed and rate of metal removal

Page 119: Theory of metal cutting-module II

119

Effects of Temperature and Friction

• Temperature of metal immediately ahead of cutting tool comes close to melting temperature of metal being cut.

• Greatest heat generated when ductile material of high tensile strength is cut.

• Lowest heat generated when soft material of low tensile strength is cut.

• Maximum temperature attained during cutting action.

– affects cutting-tool life, quality of surface finish, rate of production and accuracy of work piece.

Page 120: Theory of metal cutting-module II

120

Friction• Kept low as possible for efficient cutting action

• Increasing coefficient of friction gives greater possibility of built-up edge forming

– Larger built-up edge, more friction

– Results in breakdown of cutting edge and poor surface finish

• Can reduce friction at chip-tool interface and help maintain efficient cutting temperatures if use good supply of cutting fluid.

Page 121: Theory of metal cutting-module II

121

Factors Affecting Surface Finish

• Feed rate

• Nose radius of tool

• Cutting speed

• Rigidity of machining operation

• Temperature generated during machining process

Page 122: Theory of metal cutting-module II

122

Surface Finish• Direct relationship between temperature of work piece

and quality of surface finish

– High temperature yields rough surface finish

– Metal particles tend to adhere to cutting tool and form built-up edge

• Cooling work material reduces temperature of cutting-tool edge

– Result in better surface finish