    CONTENTS

    Master die

    Wax pattern

    Spruing

    Liner

    Investing procedure

    Casting machines

    Cleaning the casting

    Causes of defective castings

    Porosity

    Conclusion

    References

  • 7/29/2019 Casting Procedures and Casting Defects

    3/70

    Definitions

    According to glossary of Prosthodontics terms (GPT-8)

    Casting(1) something that has been cast in a mold.

    (2) An object formed by the solidification of fluid that hasbeen poured or injected in to a mold.

    Sprue former- A wax, plastic, or metal pattern used toform the channel allowing molten metal to flow in the moldto make a casting.

    Investing The process of covering or enveloping wholly

    or in part , an object such as denture , tooth, wax form,crown etc. with a suitable investment material beforeprocessing or casting.

  • 7/29/2019 Casting Procedures and Casting Defects

    4/70

    Master die

    After making impression first step is die making. The mostcommonly used die materials are Type IV and Type Vimproved stones.

    Setting expansion of Type IV stone is 0.1% and Type V is0.3%.

    To reduce setting expansion accelerator( potassium sulfate )and retarder( borax) can be added.

    Different types and methods of die making

    1 Die stoneinvestment combination2 Other die materials( acrylic, polyester and epoxy resin)

    3 Electroformed die

  • 7/29/2019 Casting Procedures and Casting Defects

    5/70

    Wax pattern

    According to American dental association specificationnumber 4, wax used for making wax pattern are divided into

    three types:

    Type A - Hard or low flow wax used in indirect technique .

    Type B Used for direct technique .

    Type C Also used for direct technique.

    To allow for a clean separation of the wax pattern from a

    gypsum die, a die lubricant must be applied to gypsumsurface prior to placement of molten wax .

    Lubricant is oil based . And excess of lubricant should not beused as it may obscure detail of die, or may get adsorbed to

    the wax pattern.

  • 7/29/2019 Casting Procedures and Casting Defects

    6/70

    Spruing the wax pattern

    Investing the wax pattern

    Burning out the wax pattern

    Casting the dental alloy

    Sandblasting the framework

    Finishing the framework

    Steps involved in a casting procedure

  • 7/29/2019 Casting Procedures and Casting Defects

    7/70

    SpruingPurpose

    To form a mount for the wax pattern and fix the pattern inspace so a mold can be made.

    To create a channel for elimination of wax during burnout.

    To form a channel for the ingress of molten alloy.

    compensate for alloy shrinkage during solidification.

    Sprue Size And Design

    Large and small inlays require sprues that are 14 gauge (4 to 5

    mm long) and 16 gauge (3 to 4 mm long), respectively.

    Large and small crowns require 10- and 12gauge sprues,

    respectively, with an average sprue length of 4 to 5 mm.

  • 7/29/2019 Casting Procedures and Casting Defects

    8/70

    Point Of Attachment

    Sprue attachment must always be made at the bulkiest

    portion of the pattern.

    a- crucible former, b-sprue, c-cavity formed

    by wax pattern after burnout, d-investment,

    e- liner, f- casting ring, g- recommended

    maximum thickness of approx. 6 mm. b/w

    the end of invested ring to provide

    pathway for gas escaping.

    The wax sprue is the most commonly used.

    A hollow-metal sprue pin is preferable to a solid metal pin.

    Plastic sprues are not recommended.

    Sprue Selection

  • 7/29/2019 Casting Procedures and Casting Defects

    9/70

    Liner The most commonly used technique to provide

    investment expansions is to line the walls of the ring with

    a ring liner.

    Traditionally, asbestos was the material of choice.

    Three types of non-asbestos ring liner materials havebeen produced:

    1. an aluminosilicate ceramic liner

    2. cellulose (paper) liner

    3. Ceramic cellulose combination

  • 7/29/2019 Casting Procedures and Casting Defects

    10/70

    Functions of ring liner1. A liner is placed inside the ring to allow lateral expansion of

    the investment.

    2. When the ring is transferred from the furnace to the castingmachine it reduces heat loss as it is thermal insulator

    3. Permits easy removal of the investment after casting.

    Three millimeters of clearance is allowed at each end of thering so the mold is sealed and anchored.

    The dry liner is tacked in position with sticky wax, and it isthen used either dry or wet.

    With a wet liner technique, the lined ring is immersed inwater for a time, and the excess water is shaken away.

    Squeezing the liner should be avoided, because this lead tovariable amounts of water removal and nonuniformexpansion.

  • 7/29/2019 Casting Procedures and Casting Defects

    11/70

    INVESTING PROCEDURE

    The wax pattern should be cleaned of any debris.

    Appropriate amount of distilled water (gypsuminvestments) or colloidal silica special liquid (phosphate

    investments) is dispensed.

    Mechanical mixing under vacuum removes air bubblescreated during mixing and evacuates any potentiallyharmful gases produced by the chemical reaction of thehigh-heat investments.

  • 7/29/2019 Casting Procedures and Casting Defects

    12/70

  • 7/29/2019 Casting Procedures and Casting Defects

    13/70

    Compensation for Shrinkage

    Two liners allow a greater setting and thermalexpansion than does a single liner.

    By varying the L/P ratio of the investment.

    Casting procedure

    Invested ring is placed in a room temp. furnace and

    heated up to

    For gypsum bonded ( hygroscopic ) ------ 468 oC

    For gypsum bonded ( thermal expansion ) ---- 650 oC

    For phosphate bonded investment -------700 - 870 oC

  • 7/29/2019 Casting Procedures and Casting Defects

    14/70

    Hygroscopic low heat technique

    In this technique compensation for shrinkage is done with :

    1. 37oc water bath expands the wax pattern.

    2. Warm water enters the mold and hygroscopic expansion

    is obtained .

    3. thermal expansion

    During this technique care must be taken to allow sufficient

    burnout time because wax is slowly eliminated at low

    temperature.

    Porosity is more in low temp. technique then high temp.

    technique

  • 7/29/2019 Casting Procedures and Casting Defects

    15/70

    The hygroscopic technique was developed for alloys with

    high gold content but there was a need for slightly moreexpansion for newer noble alloys and this addedexpansion may be obtained from :

    1. increasing the water bath temp. to 40 0c

    2. using two layer of liner.

    3. increasing the burnout temp. to a range of 600oc -650oc

  • 7/29/2019 Casting Procedures and Casting Defects

    16/70

    High heat thermal expansion technique

    This technique mainly depends on high heat burnout toobtain the required expansion.

    Gypsum investment isnt heated more than 700 0c,because above this temperature carbon react withcalcium sulfate binder & forms sulfur dioxide whichcontaminates gold casting and make them extremelybrittle.

  • 7/29/2019 Casting Procedures and Casting Defects

    17/70

    In phosphate investment expansion is obtained from :

    1. Expansion of wax pattern

    2. Setting expansion which is higher than gypsum

    investment because in phosphate investment colloidal

    silica is used as a liquid

    3. Thermal expansion which is also greater.

    A total expansion of 2% or more is required for porcelain

    bonded alloys.

  • 7/29/2019 Casting Procedures and Casting Defects

    18/70

    WAX ELIMINATION AND HEATING

    It is also advisable to begin the burnout procedurewhile the mold is still wet. Water trapped in thepores of the investment reduces the absorption ofwax, and as the water vaporizes, it flushes wax from

    the mold.

    If the burnout procedure does not immediately

    follow the investing procedure, the invested ring isplaced in a humidor at 100% humidity.

  • 7/29/2019 Casting Procedures and Casting Defects

    19/70

    Gypsum Investments

    Rapid heating can generate steam, which can causeflaking or spalling of the mold walls.

    Too many patterns in the same plane within the

    investment often cause separation of a whole section

    of investment, because the expanding wax creates

    excessive pressure over a large area.

    Too rapid a heating rate may also cause cracking of the

    investment

  • 7/29/2019 Casting Procedures and Casting Defects

    20/70

    The outside layer starts to expand thermally, resulting incompressive stress in the outside layer, whichcounteracts tensile stresses in the middle regions of themold.

    Such a stress distribution causes the brittle investment tocrack from the interior outwardly in the form of radialcracks. These cracks, in turn, produce a casting with fins

    or spine.

    Fins on the surface of a casting that formedas a result of cracks in the investment

    before casting of the metal.

  • 7/29/2019 Casting Procedures and Casting Defects

    21/70

    Phosphate Investments

    Phosphate investments obtain their expansion from thefollowing sources:

    Expansion of the wax pattern this is considerable becausethe setting reaction raises the mold temperaturesubstantially.

    Setting expansion this is usually higher than in gypsuminvestments, especially because special liquids are used toenhance such expansion.

    Thermal expansion

    this is greater when taken totemperatures higher than those used for gypsum-bondedinvestments.

  • 7/29/2019 Casting Procedures and Casting Defects

    22/70

    The usual burnout temperatures for phosphate-bondedinvestments range from 750 to 1030 C.

    Highest temperatures are required for base metal alloys.

    The heating rate is usually slow to 315 C and is quite rapidthereafter, reaching completion after a hold at the uppertemperature for 30 minutes.

    To save time, the metal ring is being replaced with a plastic

    ring that is tapered so that once the investment has set, itcan be pushed out of the ring, held for a specified time toensure complete setting, and then placed directly into thehot furnace.

  • 7/29/2019 Casting Procedures and Casting Defects

    23/70

    Time gap before doing Casting

    The investment contracts thermally as it cool.

    Under average conditions of casting, approximately 1minute can pass without a noticeable loss in dimension.

    In the low-heat casting technique, the temperaturegradient between the investment mold and the room isnot as great as that employed with the high-heattechnique.

    Alloy should be cast soon after removal of the ring fromthe oven; otherwise a significant variation from thedesired casting dimensions may occur.

  • 7/29/2019 Casting Procedures and Casting Defects

    24/70

    CASTING MACHINES

    Alloys are melted in one of the four following ways,depending on various types of casting machines:

    The alloy is melted in a separate crucible by a torchflame and is cast into the mold by centrifugal force.

    The alloy is melted electrically by a resistance heating orinduction furnace, then cast into the mold centrifugallyby motor or spring action.

    The alloy is melted by induction heating, then cast into

    the mold centrifugally by motor or spring action.

    The alloy is vacuum arc melted and cast by pressure inan argon atmosphere.

  • 7/29/2019 Casting Procedures and Casting Defects

    25/70

    Torch Melting/Centrifugal Casting Machine The alloy is melted by a torch flame

    in a glazed ceramic crucibleattached to the "broken arm" of thecasting machine.

    The broken arm feature accelerates

    the initial rotational speed of thecrucible and casting ring, thusincreasing the linear speed of theliquid casting alloy as it moves intoand through the mold.

    Once the metal has reached thecasting temperature and the heatedcasting ring is in position, themachine is released and the spring

    triggers the rotational motion.

  • 7/29/2019 Casting Procedures and Casting Defects

    26/70

    METAL FLOWS IN TO THE MOLD

  • 7/29/2019 Casting Procedures and Casting Defects

    27/70

    As metal fills hydrostatic pressure gradient developsalong the length of the casting. The pressure gradientfrom the tip of the casting to the bottom surface is

    quite sharp and parabolic in form, reaching zero atthe button surface.

    Pressure gradient at the moment beforesolidification reaches is about 0.21 to 0.28 MPa (30

    to 40 psi) at the tip of the casting.There is also a gradient in the heat transfer rate suchthat the greatest rate of heat transfer to the mold isat the high pressure end of the gradient (i.e., the tipof the casting).

    Because this end also is frequently the sharp edge ofthe margin of a crown, there is further assurancethat the solidification progresses from the thinmargin edge to the button surface.

  • 7/29/2019 Casting Procedures and Casting Defects

    28/70

    Electrical Resistance-Heated Casting Machine Current is passed through a resistance heating

    conductor, and automatic melting of the alloy occurs in

    a graphite or ceramic crucible.

    Advantages:

    Used for metal-ceramic prostheses, which are alloyedwith base metals in trace amounts that tend to oxidizeon overheating.

    The crucible in the furnace is located flush against thecasting ring.

    Therefore the alloy button remains molten slightlylonger, again ensuring that solidification progressescompletely from the tip of the casting to the buttonsurface.

  • 7/29/2019 Casting Procedures and Casting Defects

    29/70

    Induction MeltingMachineAlloy is melted by an induction field that

    develops within a crucible surrounded bywater cooled metal tubing.

    The electric induction furnace is atransformer in which an alternating currentflows through the primary winding coil andgenerates a variable magnetic field in thelocation of the alloy to be melted in acrucible.

    Once the alloy reaches the casting

    temperature in air or in vacuum, it is forcedinto the mold by centrifugal force, by airpressure, or by vacuum.

    Used for melting base metal alloys.

  • 7/29/2019 Casting Procedures and Casting Defects

    30/70

    Direct Current Arc Melting Machine The direct current arc is produced between two

    electrodes: the alloy and the water cooled tungstenelectrode.

    The temperature within the arc exceeds 4000C, andthe alloy melts very quickly.

    This method has a high risk for overheating the alloy,and damage may result after only a few seconds ofprolonged heating.

  • 7/29/2019 Casting Procedures and Casting Defects

    31/70

    Vacuum or Pressure Assisted Casting Machine The molten alloy is heated to the casting temperature,

    drawn into the evacuated mold by gravity or vacuum,and subjected to additional pressure to force the alloy

    into the mold.

    For Titanium and Titanium alloys, vacuum arc heated

    argon pressure casting machines are required.

  • 7/29/2019 Casting Procedures and Casting Defects

    32/70

    Casting Crucibles

    Four types of casting crucibles are:

    Clay, Carbon,

    Quartz, and

    Zirconium-alumina

    Clay crucibles are appropriate for many of the crownand bridge alloys, such as the high noble and noble

    types.

    Carbon crucibles can be used not only for high noblecrown and bridge alloys but also-for the higher-fusing,

    gold-based metal-ceramic alloys.

  • 7/29/2019 Casting Procedures and Casting Defects

    33/70

    Torch Melting of Noble Metal Alloy

    Fuel used is a mixture of natural or artificial gas and air,

    oxygen-air and acetylene can also be used. When the reducing zone is in contact, the surface of the

    gold alloy is bright and mirror like.

  • 7/29/2019 Casting Procedures and Casting Defects

    34/70

    FLAME

  • 7/29/2019 Casting Procedures and Casting Defects

    35/70

    Mirror like surface of the metal indicates proper fusion. B, Cloudy surface

    indicates surface oxidation by improper positioning of the torch flame.

    When the oxidizing portion of the flame is in contact with

    the alloy, there is a dull film of "dross" developed over the

    surface.

    The alloy first appears to be spongy, and then smallglobules of fused alloy appear.

  • 7/29/2019 Casting Procedures and Casting Defects

    36/70

    The molten alloy soon assumes a spheroidal shape.

    At the proper casting temperature, the molten alloy is

    light orange and tends to spin or follow the flame whenthe latter is moved slightly.

    At this point, the alloy should be approximately 38 to66 C above its liquidus temperature.

    The casting should be made immediately when the

    proper temperature is reached.

  • 7/29/2019 Casting Procedures and Casting Defects

    37/70

    HEAT TREATMENT

    Heat treatment is helpful in finishing margins.

    To adequately resist excessive wear, however, therestoration must be returned to a hardened state prior toits clinical use.

    It is done for all gold alloys.

    Softening heat treatment: consist of heating the alloy to

    700C and maintaining that temperature for

    approximately 15 minutes, followed by quenching in room

    temperature water.

  • 7/29/2019 Casting Procedures and Casting Defects

    38/70

    May be conducted in either of two ways :

    Heat soaking at a constant temperature of

    approximately 450C for 15 minutes.

    Slow cooling from 450C 250C over a period of 15

    minutes, followed by quenching in water.

    CLEANING THE CASTING

  • 7/29/2019 Casting Procedures and Casting Defects

    39/70

    CLEANING THE CASTING

    Two advantages are gained in quenching:

    (1) The noble metal alloy is left in an annealed condition for

    burnishing, polishing, and similar procedures,(2) When the water contacts the hot investment, a violent reaction

    ensues, resulting in a soft, granular investment that is easilyremoved.

    The surface of the casting appears dark with oxides and tarnish.

    Such a surface film can be removed by a process known aspickling,which consists of heating the discolored casting in anacid.

    One of the best pickling solutions for gypsum-bonded

    investments is a 50% hydrochloric acidsolution.

  • 7/29/2019 Casting Procedures and Casting Defects

    40/70

    The disadvantage of hydrochloric acid is that the fumes from the acid are likely

    to corrode laboratory metal furnishings.

    The pickling process can be performed ultrasonically while the prosthesis is

    sealed in a Teflon container.

    A solution of 50% sulfuric acid may also be more advantageous in this respect.

    Cold hydrofluoric acid dissolves the silica refractory quite well without damageto a gold-based or a palladium-silver alloy.

    Base metal alloys require a light Sandblasting,

    usually with fine alumina.

  • 7/29/2019 Casting Procedures and Casting Defects

    41/70

    Selecast System Titanium casting

    system for dentistry

    Designed as full-automatic operation

    It includes LCD operation panel

    It includes Inverter-motor for more stability of turn-table.

    There more large size vacuum pump

    The electric devices have wider margin to its limit value, it

    means to be more safety.

  • 7/29/2019 Casting Procedures and Casting Defects

    42/70

    Characteristics

    In 'SPIN CAST

    METHOD' pores are

    scarcely formed, since

    mold rotates (with

    3,000 r.p.m.) before

    casting.

    Structure

    http://www.selec-inc.com/eng/Selecast%20from%20selec%20co.,%20Ltd.
  • 7/29/2019 Casting Procedures and Casting Defects

    43/70

    Structure

    It has a vacuum chamber in its upper body, which consists of argonarc melting system and centrifugal casting system.

    The body contains vaccum pump, high-voltage electrode formelting, turn-table rotary motor, bulbs and control system whichcovers all of the device.

    When 'POWER' button is pushed and touch to auto start, the

    chamber is evacuated and argon gas flows in it.

    Arc melting with tungsten electrode, titanium ingot in cruciblemelts down in argon atmosphere.

    After the rotary speed of the mold (which is horizontally spun) getshigher than fixed, molten titanium is poured into the gate from thetilting crucible

    Casting method Horizontal centrifugal

  • 7/29/2019 Casting Procedures and Casting Defects

    44/70

    Casting method Horizontal-centrifugal

    casting with tilting - type

    crucible

    Melting method After vacuumed, electric are

    melting in argon atmosphere

    Melting ability Max.41g

    (pure titanium and titanium

    alloy)

    Electric control Automationexhaustion - feeding of

    argon - spinning of mold -

    melting - casting

    Chamber volume 14.6 liters

    Revolution of

    mold

    Max. 3,000 R.P.M

    Size (outward) W510 * D725 * H 1,130

    (mm)

    Weight 220kg

  • 7/29/2019 Casting Procedures and Casting Defects

    45/70

    CAUSES OF DEFECTIVE CASTINGS

    Defects in castings can be classified under four headings:

    (1) Distortion

    (2) Surface roughness and irregularities

    (3) Porosity

    (4) Incomplete or missing details

    Di i

  • 7/29/2019 Casting Procedures and Casting Defects

    46/70

    Distortion Is probably related to distortion of the wax pattern.

    This type of distortion can be minimized by proper

    manipulation of the wax and handling of the pattern.

    Distortion of the wax pattern occurs as the investment

    hardens around it.

    The setting and hygroscopic expansions of the investmentmay produce a non-uniform expansion of the walls of thepattern.

    The gingival margins are forced apart by the moldexpansion, whereas the solid occlusal bar of wax resists

    expansion during the early stages of setting. The lesser the setting expansion of the investment, the less

    the distortion.

    S f R h I l iti d Di l ti

  • 7/29/2019 Casting Procedures and Casting Defects

    47/70

    Surface Roughness, Irregularities, and Discoloration

    Surface roughness is defined as relatively finely spared

    surface imperfections whose height, width, and direction

    establish the predominant surface pattern.

    Surface irregularities are isolated imperfections, such as

    nodules, that are not characteristic of the entire surface

    area.

    Surface irregularities on anexperimental casting caused byair bubbles (A), water film (B)and inclusion of foreign body (C)

    bbl

  • 7/29/2019 Casting Procedures and Casting Defects

    48/70

    Air Bubbles Small nodules on a casting are caused by air bubbles that

    become attached to the pattern during or subsequent to

    the investing procedure. For nodules on margins or on internal surfaces removal of

    these irregularities might alter the fit of the casting.

    Prevention

    The use of a mechanical mixer with vibration both beforeand after mixing should be practiced routinely.

    The wetting agent be applied in a thin layer. It is best to air dry the wetting agent, because any excess

    liquid dilutes the investment, possibly producing surfaceirregularities on the casting.

    W Fil

  • 7/29/2019 Casting Procedures and Casting Defects

    49/70

    Water FilmsWax is repellent to water and if the investmentbecomes separated from the wax pattern in somemanner, a water film may form irregularly over thesurface.

    This type of surface irregularity appears as minute

    ridges or veins on the surface.

    Too high an L/P ratio may also produce these surfaceirregularities.

    A wetting agent is of aid in the prevention of suchirregularities.

    Under Heating

  • 7/29/2019 Casting Procedures and Casting Defects

    50/70

    Under Heating

    Incomplete elimination of wax residues may occurparticularly with the low-temperature investment

    techniques.

    Voids or porosity may occur in the casting from thegases formed when the hot alloy comes in contact with

    the carbon residues.

    The casting may also be covered with a tenaciouscarbon coating that is virtually impossible to removeby pickling.

    P l d H ti

  • 7/29/2019 Casting Procedures and Casting Defects

    51/70

    Prolonged Heating

    If the high-heat casting technique is used, a prolongedheating of the mold at the casting temperature is likely tocause a disintegration of the gypsum-bonded investment,and the walls of the mold are roughened as a result.

    The products of decomposition are sulfur compounds thatmay contaminate the alloy to the extent that the surface

    texture is affected.

    Temperature of the Alloy

    If an alloy is heated to too high a temperature beforecasting, the surface of the investment is likely to beattacked, and a surface roughness may result.

    Casting Pressure

  • 7/29/2019 Casting Procedures and Casting Defects

    52/70

    Casting Pressure Too high a pressure during casting can produce a rough

    surface on the casting.

    A gauge pressure of 0.10 to 0.14 MPa in an air pressurecasting machine orthree tofour turns of the spring in anaverage type of centrifugal casting machine is sufficient forsmall castings.

    Composition of the Investment

    The ratio of the binder to the quartz influences the surface

    texture of the casting.

    A coarse silica causes a surface roughness.

    Foreign Bodies

  • 7/29/2019 Casting Procedures and Casting Defects

    53/70

    Foreign Bodies

    A rough crucible former with investment clinging to

    it may roughen the investment on its removal sothat bits of investment are carried into the moldwith the molten alloy.

    Carelessness in the removal of the sprue former canalso be a cause for it.

    Casting that shows sharp, well defined deficienciesindicates the presence of some foreign particles inthe mold, such as pieces of investment and bits ofcarbon from a flux.

    Bright appearing concavities may be the result of

  • 7/29/2019 Casting Procedures and Casting Defects

    54/70

    Bright appearing concavities may be the result offlux being carried into the mold with the metal.

    Surface discoloration and roughness can resultfrom sulfur contamination, either frominvestment breakdown at elevated temperatures

    or from a high sulfur content of the torch flame.

    The interaction of the molten alloy with sulfur

    produces a black or grey layer on the surface ofgold alloys that is brittle and does not cleanreadily during pickling.

    I t f M lt All

  • 7/29/2019 Casting Procedures and Casting Defects

    55/70

    Impact of Molten Alloy The molten alloy may fracture or abrade the mold

    surface on impact, regardless of its bulk.

    The direction of the sprue former should be such thatthe molten gold alloy does not strike a weak portion ofthe mold surface.

    It is unfortunate that sometimes the abraded area issmooth so that it cannot be detected on the surface ofthe casting.

    Such a depression in the mold is reflected as a raisedarea on the casting.

    Pattern Position

  • 7/29/2019 Casting Procedures and Casting Defects

    56/70

    Pattern Position

    If several patterns are invested in the same ring, theyshould not be placed too close together.

    Positioning too many patterns in the same plane in themold should be avoided.

    The expansion of wax is much greater than that of theinvestment, causing breakdown or cracking of theinvestment if the spacing between patterns is less than 3

    mm.

    Carbon Inclusions

  • 7/29/2019 Casting Procedures and Casting Defects

    57/70

    Carbon Inclusions

    Carbon, as from a crucible, an improperly adjustedtorch, or a carbon containing investment, can beabsorbed by the alloy during casting.

    These particles may lead to the formation of carbidesor even create visible carbon inclusions.

    Porosity

  • 7/29/2019 Casting Procedures and Casting Defects

    58/70

    Porosity Porosities in noble metal alloy castings may be classified as

    follows:

    I. Solidification defects

    A. Localized shrinkage porosity

    B. Microporosity

    II. Trapped gases

    A. Pinhole porosity

    B. Gas inclusionsC. Subsurface porosity

    III. Residual air

  • 7/29/2019 Casting Procedures and Casting Defects

    59/70

    Porosities

    Solidification

    DefectsTrapped gases Residual Air

    Localized

    ShrinkageMicroporosity

    Pinhole

    Porosity

    Gas

    Inclusions

    Subsurface

    Porosity

  • 7/29/2019 Casting Procedures and Casting Defects

    60/70

    Localized shrinkage is generally caused by premature

    termination of the flow of molten metal during solidification.

    The linear contraction of noble metal alloys in changing from

    a liquid to solid is at least 1.25%.

    Continual feeding of molten metal through the sprue must

    occur to make up for the shrinkage of metal volume duringsolidification.

    Porosity in pontic area is caused by its ability to retain heatbecause of its bulk.

    This problem can be solved by attaching one or more smallgauge sprues called as chill setsprues.

    These act as cooling pins to carry away heat from pontic.

    Void may also occur externally, usually in the interior of a

  • 7/29/2019 Casting Procedures and Casting Defects

    61/70

    Void may also occur externally, usually in the interior of acrown near the area of the sprue, if a hot spot has beencreated by the hot metal impinging from the sprue channelon a point of the mold wall.

    This hot spot causes the local region to freeze last andresults in what is called suck-back porosity.

    Suck-back porosity often occurs at an occlusoaxial line angle

    or incisoaxial line angle that is not well rounded.

    Suck-back porosity can be eliminated by flaring the point of

    sprue attachment and reducing the mold melt temperature

    differential, that is, lowering the casting temperature by

    about 30 C.

  • 7/29/2019 Casting Procedures and Casting Defects

    62/70

    Microporosityalso occurs from solidification shrinkage but isgenerally present in fine grain alloy castings when thesolidification is too rapid for the micro voids to segregate to

    the liquid pool.

    Pinholeand the Gas inclusionporositiesare related to theentrapment of gas during solidification.

    The gas inclusion porosities are usually much larger than

    pinhole porosity.

    On solidification, the absorbed gases are expelled and pinhole

    porosity results.

  • 7/29/2019 Casting Procedures and Casting Defects

    63/70

    Larger spherical porosities can be caused by gas occludedfrom a poorly adjusted torch flame, or by use of the mixing oroxidizing zones of the flame rather than the reducing zone.

    These types of porosity can be minimized by pre- melting thegold alloy on a graphite crucible or a graphite block, if thealloy has been used before, and by correctly adjusting andpositioning the torch flame during melting.

    Subsurface porosityoccurs on occasion, the reasons for suchvoids have not been completely established.

    They may be caused by the simultaneous nucleation of solidgrains and gas bubbles at the first moment that the alloyfreezes at the mold walls.

    This type of porosity can be diminished by controlling the

    rate at which the molten metal enters the mold.

    Entrapped air porosity on the inner surface of the casting,

  • 7/29/2019 Casting Procedures and Casting Defects

    64/70

    pp p y g,sometimes referred to as back-pressure porosity, canproduce large concave depressions.

    This is caused by the inability of the air in the mold to escapethrough the pores in the investment or by the pressuregradient that displaces the air pocket toward the end of theinvestment via the molten sprue and button.

    The entrapment is frequently found in a "pocket" at thecavity surface of a crown or mesio-occlusal-distal casting.

  • 7/29/2019 Casting Procedures and Casting Defects

    65/70

    Incomplete Casting

  • 7/29/2019 Casting Procedures and Casting Defects

    66/70

    Incomplete Casting Occasionally, only a partially complete casting, or perhaps no

    casting at all, is found.

    Cause is that the molten alloy has been prevented in somemanner, from completely filling the mold.

    CAUSES

  • 7/29/2019 Casting Procedures and Casting Defects

    67/70

    The first consideration- insufficient venting, is directly related tothe back pressure exerted by the air in the mold. If the air cannotbe vented quickly, the molten alloy does not fill the mold before itsolidifies.

    In such a case, the magnitude of the casting pressure should be

    suspected. If insufficient casting pressure is used, the back pressure cannot

    be overcome.

    Furthermore, the pressure should be applied for at least 4seconds.

    The mold is filled and the alloy is solidified in 1 second or less; yetit is quite soft during the early stages. The pressure should bemaintained for a few seconds beyond this point.

    CAUSES

    A second common cause for an incomplete casting is

  • 7/29/2019 Casting Procedures and Casting Defects

    68/70

    incomplete elimination of wax residues from the mold.

    If too many products of combustion remain in the mold, thepores in the investment may become filled so that the aircannot be vented completely.

    If moisture or particles of wax remain, the contact of the

    molten ; alloy with these foreign substances produces anexplosion that may produce sufficient back pressure toprevent the mold from being filled.

    CONCLUSION

  • 7/29/2019 Casting Procedures and Casting Defects

    69/70

    CONCLUSION

    Production of an accurate casting requires development

    of a precise casting procedure.

    Many problems can be encountered during castingprocedure resulting defects in final castings.

    Adherence to the casting procedures described will aid inthe production of clean, well fitting castings.

    REFERENCES

  • 7/29/2019 Casting Procedures and Casting Defects

    70/70

    Science of dental materials- Anusavice, 11th Edn

    Restorative dental materials - Craig,10th Edn.

    Applied dental Materials -John F. Mc Cabe,7th Edn. Dental materials, Properties & Manipulation -Robert G. Craig et.al,

    5th Edn.

    Journal of Prosthet Dent. 2002; 87:94-98.

    Journal of Prosthet Dent. 1988; 80: 691-698.

    Journal of Prosthet Dent. 1987; 85: 1-5.

    Journal of Prosthet Dent. 1986; 56: 507-509.

    Journal of Prosthet Dent. 1982; 48: 99-101.

    Dental materials. 1987; 3: 125-130.

    Dental materials. 1993; 9: 177-181.

    Intl Journal Prosthodont. 1991;4:152-158.

    J Dent Research. 1990; 69: 67-68.